SlideShare a Scribd company logo
1 of 178
CASTING PROCEDURES
Presented by:
Dr. Jehan Dordi
I year MDS
1
CONTENTS
• Introduction
• Sprue and Spruing
• Crucible Former
• Casting Ring
• Casting Ring Liner
• Investing
• Shrinkage Compensation
• Burnout Procedure
• Casting machines
• Casting Crucibles
• Flux in Casting
• Heat treatment
2
• Casting Procedures
• Divesting & Cleaning the casting
• Finishing and polishing
• Degassing Ceramo-metal casting
• Casting defects
• Review of Literature
• References
3
INTRODUCTION
4
Terminology
• Casting: It is defined as something that has been cast in a mold; an object formed by the
solidification of a fluid that has been cast into a refractory mould (GPT-9).
5
3000 B.C- Copper was cast by Mesopotamian's
2500 B.C- Dental prosthesis fabricated from gold wire was found in Egypt
500 B.C.- Etruscans made bridges of soldered gold bands
1571- Benevento had done casting of both gold and bronze
1897- Phil brook described a method of casting metal in mould formed from a wax
pattern for posterior tooth
1907- Taggart devised a practically useful casting machine
1928- The low heat casting technique was published by Coleman
1930- Carl Scheu, discovered the phenomena known as Hygroscopic Setting Expansion
1945- George D. Estes introduced the vacuum investing technique to prevent formation
of air bubbles on surface of wax
1959- Strickland et al stated importance of type, shape & direction other than size of
sprue
1959- Peyton stated tar flaring should occur at the sprue/ wax pattern junction 6
The Lost Wax Process
• The casting procedure by lost wax technique
was introduced by Dr. William H. Taggart.
• He introduced this technique and the casting
machine in 1907 before the New York
Odontological Group .
• It soon led to the casting of inlays, onlays,
clowns, fixed partial dentures (TPDs), and
frameworks for removable partial dentures.
Blowpipe
Mould
Compressed air cylinder
7
Steps In Casting Procedure
• Tooth/ teeth preparation
• Impression
• Die Preparation
• Wax pattern fabrication
• Spruing
• Investing procedure
• Burn out procedure
• Casting
• Divesting & Cleaning of the casting
• Finishing of the casting
8
SPRUE & SPRUING
9
Sprue
• It is the channel or hole through which plastic or metal is poured or cast into a gate or reservoir
and then into a mould. (GPT-9)
Wax pattern attached to the crucible former with a sprue ready for investing. A ring liner is in place. 10
Types of Sprue
• According to material used:
• Wax sprue former (for large restorations E.g.. RPD
frameworks)
• Plastic/Resin sprue former (smaller restorations)
• Metal sprue ( smaller restorations E.g.. Crown)
• According to process:
• Prefabricated
• Custom made
• According to shape:
• Solid
• Hollow (Round)
• According to the diameter of teeth:
• For molars: 2.5mm (10-gauge)
• For anteriors and pre-molars: 2.0mm (12-gauge)
11
Materials Used In Sprue
• Special wax supplied as rope form (rolls) of different diameters (gauges) for selection.
• Hollow stainless steel wires of different diameters and lengths.
• These are to be coated with thin layer of inlay wax by dipping in molten wax.
• This is done for easy removal of sprue former after setting of investment.
12
Length & Diameter of The Sprue
• The length of the sprue former should be adjusted so that the pattern is approximately 6 mm
from the open end of the ring.
• The sprue former should be atleast 1.7mm in diameter unless the pattern is extremely small.
• Sprue formers upto 2.5mm in diameter is used for very large patterns and bulky full crowns.
13
Sprue Former Direction
• It is attached at 45 degrees to the walls
of the mould, which decreases the
turbulence of molten alloy.
14
Spruing Principles And Technique
• The first step in the production of refractory mould is termed as spruing the pattern, whereby the
wax pattern is attached to conical base by extension of wax, plastic, or metal.
• This connector is known as sprue former, which should be properly selected in respect to size
and configuration.
15
Location Of Sprue
• Sprue is attached to the bulkiest, non-critical part of the pattern.
• Away from the margins and occlusal contacts.
• Normally it is attached to largest non-functional cusp used.
Wrong Correct
16
Types of Spruing
• Direct spruing: Sprue former provides direct connection between
pattern area and the crucible former.
• A basic weakness of direct spruing is the potential for suck back
porosity at the junction of restoration and the sprue.
• Indirect spruing: It uses the same basic principal of spruing. But the
only difference lies in attachment of 3 running horizontal bars. The
whole indirect sprue complex consists of 3 parts:
1. Feeder sprue
2. Horizontal running bar
3. 6 or 8 gauge sprue former
17
Spruing The Pattern
• Selection of sprue former depends on
1. type and size of the pattern and
2. the size of the ring used.
• Long and thin sprue formers cause internal porosity.
• This maybe overcome by using a reservoir or larger sprue.
• Reservoir must have greater bulk than the adjacent portion of the pattern into which the sprue
former is inserted.
Reservoir
18
Wax sprue-former length is checked before attachment to
ensure that pattern is at least 3 to 6 mm from end of ring.
19
• Any overheating of the wax could distort the pattern and hence hollow metal/plastic sprue
formers are preferred, since they hold less heat than a solid sprue former.
• The sprue former should be smooth and produce no sharp angles at the juncture of the wax
pattern or the crucible former.
Sprue former placement should provide smooth-flowing
entry of gold into mold (arrows), with no sharp angles.
Sprue former
20
• Prefabricated sprue formers are available in a variety of
sizes and configurations.
• These plastic sprue formers are more rigid and
decreases the chances of distorting the pattern.
• A three-unit bridge and sprues with the “gate”
technique, using prefabricated plastic formers is
particularly useful for long-span multiple castings.
Prefabricated plastic sprue formers
Three-unit bridge and sprues with "gate" technique,
using prefabricated plastic sprue former
21
• Poor sprue designs can result in poor castings.
• The sprue former must provide a proper in gate,
allowing for smooth unobstructed flow of the
molten gold into the mould.
Poor sprue designs such as these can lead to casting failure.
22
Spruing Metal-Ceramic Units
• For small crowns a short, 8-gauge wax sprue
former should be placed on the incisal edge so
that the alloy may flow directly into the thinnest
section of the casting.
• The investment mold is generally about 1000° F
(540°C) cooler than the molten alloy, and
solidification occurs very quickly.
Small units are easily cast by attaching short 6- or 8-
gauge wax sprue former at incisal tip of wax pattern.
23
• Movement of the liquid metal to the most distal margins
of the casting must not be obstructed.
• There should always be sufficient bulk of the sprue to
allow for contraction of the metal during solidification
without introduction of shrinkage porosity.
• For larger castings (e.g., posterior crowns or small bridge
units) an additional auxiliary sprue may be placed to
facilitate filling the mould.
Incomplete casting caused by excessively thin
wax patterns and obstruction of gold flow in
facial area of coping.
24
• Small-diameter primary or auxiliary sprue formers attached to thicker sections of
the casting will often cause shrinkage porosity.
(A) Small primary sprue formers can create shrinkage porosity in casting.
(B) Very thin auxiliary sprues can create regions of porosity in thicker sections of larger castings.
25
• Large units are best sprued by the “gate”
method, whereby a series of short 8-gauge wax
sprue formers are attached to a continuous 6- or
8-gauge “ runner bar’ of wax or (preferably)
plastic.
1. "Gate” spruing.
A. Six- or eight-gauge sprue formers
B. runner bar, 6-gauge or larger
C. feeder sprues
D. crucible former.
2 and 3, Four-unit bridge to be cast using prefabricated plastic "gate”
sprue former. These rigid patterns help minimize wax distortion during
investing procedures. 26
• This runner bar in turn is attached to the crucible former by two or more large sprue formers,
providing:
1. A minimum of distortion of the wax pattern,
2. A fairly uniform reservoir of metal near the entire casting, and
3. Even distribution of the alloy to all parts of the casting to minimize porosity.
• For large castings, it is critical that the spruing arrangement provide a reservoir of metal that is
external to the dental unit but positioned at the heat center of the investment mould.
• Generally the alloy immediately adjacent to the walls of the mould will solidify first, the
exposed surface of the button will solidify second, and the alloy internal to the mold will cool
last. 27
• If bulky pontics are placed at the heat center of the
mould without a reservoir, porosity is very likely to
occur in the pontic itself, resulting in a weak bridge.
• Where a dental casting contains both thick and thin
elements, porosity can be minimized by the addition
of chill vents.
• Chill vents accelerate the cooling of the pontic
relative to the parts of the casting external to the
dental unit itself.
Addition of chill vents to bulky dental units may
speed solidification and minimize porosity in the
thick pontic or connector areas.
Venting
28
Spruing Of Cast Partial Framework Pattern
• Spruing for casting of removable partial dentures involves a large quantity of metal, so special
attention must be given to points of attachment, directions of the sprues, and the direction of
flow of the molten metal.
• A heavy sprue is an additional aid for offsetting the shrinkage.
• It acts as a reservoir for the casting because its bulk remains molten longer than the rest of the
casting and supplies molten metal to those areas that solidify and shrink first.
29
• Mandibular casts are usually sprued through a
hole in the center of the cast because it is easier
to attach the sprue leads.
• Maxillary casts are sprued the same way if the
shape of the casting permits; otherwise, they are
sprued from above.
• Main and auxiliary sprues are attached to the
central sprue approximately 7 mm below the tip
of the central sprue.
Wax pattern, not cast, is at least 7 mm from casting ring.
A, Maxillary wax-up showing clearance.
B, Mandibular wax-up centered in ring.
30
Procedure:
• Check the size of the investment cast in the investment
flask.
• When the wax pattern, is centered in the ring there should
be at least 7-mm clearance between the wax pattern and
the side of the ring.
• Cut a 7-mm hole through the base of the cast in the center
of the wax-up.
• The hole can be started with a bur and completed with a
knife blade.
31
• Soften half a sheet of baseplate wax.
Lay a straight hand-piece fissure bur
on the edge of the wax, and roll the
wax in a rod large enough to just pass
through the hole in the base of the
cast.
A, Straight hand-piece fissure bur is laid on edge of half sheet of softened baseplate wax
B, Wax is rolled around it to form rod large enough to just pass through hole in cast
C, Wax sprue cone completed.
32
• Push the wax rod through the base of the
refractory cast until it protrudes from the
other side about 10 mm.
• Seal the rod to the cast with wax on both sides
of the cast.
• The rod protruding through the bottom of the
cast will act as a handle during the investment
procedure.
33
• Use 8 or 10 gauge round wax for sprue leads on
mandibular casts, and lay them directly on the surface of
the cast.
• Attach one end to the central sprue and the other to the
bottom edge of the major connector.
• An auxiliary lead is usually made of 14-gauge round
sprue wax and is attached to the central sprue on the
same level as the main sprues.
• It should run as straight as possible and attach to the
minor connector on the molar just below the occlusal rest
or to the distal portion of the denture base.
34
• Six-gauge half-round wax is most often used for sprue
leads when spruing maxillary cast wax-ups.
• Reinforce and smooth all junctions between the sprues
and the framework patterns, and they are ready for
investing
35
CRUCIBLE FORMER
36
Crucible Former
• The base to which a sprue former is attached while the wax pattern is being invested in
refractory investment; a convex rubber, plastic, or metal base that forms a concave depression or
crucible in the refractory investment. (GPT-9)
• The sprue is attached to a crucible former, usually made of rubber, which serves as a base for
the casting ring during investing.
• The exact shape of the crucible former depends on the type of ring and casting machine used.
• With most modern machines, the crucible former is tall, to allow use of a short sprue and also to
enable the pattern to be positioned near the end of the casting ring.
Rubber crucible formers and
corresponding casting rings.
37
CASTING RING
38
Casting Ring
• Casting ring is a metal or silicone tube in which a refractory
mold is made for casting dental restorations (GPT-9).
• Investment material is poured in the casting ring and allowed
to set around wax pattern.
• Types of the casting ring:
1. Rubber ring
2. Metal ring
39
TYPES OF RING
ACCORDING TO
SHAPE
Round
Oval
COMPLETE RING
Rigid
Flexible
SPLIT RING
Metal
Plastic
40
CASTING RING LINER
41
Casting Ring Liner
• Casting ring liners are the materials used to line casting ring so that during heating and
expansion of the investment the compression of the liner should free the investment from the
restraint of the ring. It is placed on inner side of the casting ring.
• Types of Casting ring liner:
1. Asbestos
2. Non asbestos
i. Fibrous ceramic aluminosilicate
ii. Cellulose
iii. Ceramic- Cellulose
42
• The functions of liners are as follows:
• To allow enough lateral expansion of mould (investment), during setting or heating.
• Longer longitudinal expansion is reduced by adhesion of investment at the ends (3mm
space). This minimizes the distortion.
• When the ring is transferred from furnace to the casting machine it reduces the heat loss as it
a thermal insulator.
• Permits easy separation of the investment from the ring after casting process is over.
43
• Formerly asbestos sheet liners were laid inside
the casting ring leaving about 3mm at the ends.
• Due to health hazards of inhaling asbestos dust
or vapours which is carcinogenic, now cellulose
or alumina silicate ceramic liners are used.
Casting Ring Liner
44
• If wetted these liners provide some extra water for the Hygroscopic Setting Expansion
(HSE) of mould. Two or three layers give higher HSE of the mould laterally.
• Split casting rings or plastic casting rings are used to get adequate lateral expansions
specially for high fusing alloy.
• In base metal alloy casting procedures ring-less casting investment is done.
45
Ring-Less Casting System
• A ring-less casting system provides maximum expansion of
the investment.
• This system, is called the Power Cast ring-less system
(Whip-Mix Corporation, Louisville, USA), consists of three
sizes of rings and formers, preformed wax sprues and shapes,
investments powder and a special investment liquid.
• The tapered plastic rings allow for removal of the investment
mould after the material has set.
• This system is suited for casting of alloys that require greater
mould expansion than traditional gold based alloys.
Crucible formers and cone-shaped plastic rings for a
ringless investment technique in casting. The crucible
former and plastic ring are removed before wax
elimination, which leaves the invested wax pattern. The
systems are designed to achieve expansion that is
unrestricted by a metal ring.
46
INVESTING
47
Investing
• Investing: the process of covering or enveloping, wholly or in part, an
object such as a denture, tooth, wax form, crown, etc., with a suitable
investment material before processing, soldering, or casting. (GPT-9)
48
3 types of investments materials available:
• Gypsum bonded investments:
• For conventional casting of gold alloy inlays,
• Onlays,
• Crowns & FPD’s.
• Phosphate bonded investments:
• For metal ceramic restorations
• Pressable ceramics & for base metal alloys.
• Ethyl- silicate bonded investments:
• For casting of removable partial dentures with base metal alloy.
49
Preparatory Steps For Investing
• First of all secure the wax pattern that is made.
• A thin layer of special surfactant or wetting agents is applied, thin
layer should be maintained which otherwise collect air bubble from
the mix and cause nodule of casting.
• Cleaning the wax pattern of debris or oil is done by surfactants
which are available as:
i. Pattern Cleanser
ii. Diluted synthetic detergent solution
iii. Debbublizer
• The detergent material left behind reduces surface tension and
causes better wetting. 50
Investing Technique
• There are two methods of investing
1. Hand mixing investing method
2. Vacuum mixing and investing
51
Hand Mixing Investing Method
• Required amount of distilled water (mixture of
water + colloidal silica gel for phosphate bonded
investment) is taken in a clean flexible bowl.
• Weighed amount of powder is added and mixed
thoroughly.
• When a brush or small instrument is used to apply
the investment material to the pattern, the wet
material should be gently applied, pushed ahead of
the applicator.
(A)Paintbrush or small instrument is used to apply initial
layer of investment over pattern; this procedure decreases
chances of bubble entrapment inside pattern.
(B), Remaining investment is then poured into ring, carefully,
so as not to create voids in ring. 52
• When the pattern is completely covered in this manner, the remaining investment is poured
into the ring carefully to avoid entrapping air, and the investing procedure is completed.
• A small amount of mix is painted on the surface of wax pattern for better wetting and then
the remaining mix is vibrated into casting ring to fill completely.
• Too much vibration causes sedimentation of larger investment particles, leaving thin mix
close to the pattern, which may cause rough surface.
53
Vacuum Mixing And Investing
• Parts of machine:
1. Special investment mixing closed bowl,
2. Connection to evacuating pump,
3. A mixing pad connected to rotating shaft of an
electric motor and
4. A side platform for resting the casting ring is used.
• The proportioned material is taken in it, the speed and
time of spatulations are adjusted to get mix of
reproducible consistency.
54
• After the casting ring has been filled with the investment material, any excess
should be removed before the material sets.
• The ring is now set aside to allow the investment material to complete its setting
reaction and the accompanying setting expansion.
55
Grinding the Investment
• Carefully grind (on a model trimmer) or scrap the shiny skin off the end of the investment just
prior to burn out.
• Removes the impervious layer, opening the pores of the investment and facilitating gas release
as the alloy is cast into the mold.
• 3mm on each end is left as it serves to lock the investment within the ring & equalize radial &
axial expansion.
56
• The setting is completed in 30 to 40 minutes, at
which time it may be placed in a burnout oven to
eliminate the wax and obtain the remaining required
thermal expansion. (According to “Philips Science
of Dental Materials” the setting time is
approximately one hour.)
Before it starts to set, investment is wiped flush with
top of ring. Any scraping attempted after set may
fill in pores and inhibit gas escape from mold
during casting.
57
• When a hygroscopic technique is used, the
freshly filled investment ring is immediately
placed into a water bath for 30 minutes and kept
at 100° F (38° C).
• If metal sprue is used, it is pulled out easily, as
exothermic reaction softens the wax coating.
• The crucible formed is carefully cleaned by
removing the loosely adhering investment
particles which otherwise may fall into sprue and
block it.
Hygroscopic technique relies mainly on setting expansion to gain
proper expansion of mold. After being filled, ring is immediately
placed in constant temperature water bath at 100° F (38° C) for
at least 30 minutes.
58
SHRINKAGE COMPENSATION
59
Shrinkage compensation
• The molten alloys used for dental restorations shrink upon solidification: gold alloys by
approximately 1.5% and nickel-chromium alloys by as much as 2.4%.
• If the mold is not made correspondingly larger than the original wax pattern, the resultant
casting will be that much smaller.
• For crowns, therefore, it is necessary to compensate for the solidification shrinkage of the
specific alloy used by expanding the mold enough to at least equal the shrinkage.
Four mechanisms to produce mold expansion:
1. Setting Expansion of Investment
2. Hygroscopic Expansion
3. Wax Pattern Expansion
4. Thermal Expansion
60
• Setting Expansion: It is result of normal gypsum crystal growth. The expansion probably is
enhanced by silica particles in the investment interfering with the forming crystalline structure
of the gypsum, causing it to expand outward It occurs in small amount i.e. about 0.4% but is
partly restricted by metal investment ring.
• Hygroscopic Expansion: Maximum amount of expansion is by hygroscopic expansion. Water
bath at 38°C is used, water in bath replaces water used by hydration process. Space between
growing crystals is thus maintained. Crystals grow longer in outward direction causing
expansion of mould. About 1.2 to 2.2% hygroscopic expansion takes place. More controlled
amounts of hygroscopic expansion may be achieved by adding a measured amount of water to
the setting investment
61
• Wax pattern expansion: Expansion of the wax pattern while the investment is still fluid occurs
when the wax is warmed above the temperature at which it was formed. The low-temperature
burnout technique employs a combination of wax pattern expansion and thermal expansion of
the mold. After the investment filled ring is removed from a 100°F (38°C) water bath, the ring is
heated to only 900°F (482°C) before casting to produce the additional expansion needed.
• Thermal expansion: Thermal expansion of the investment occurs when the investment is
heated in the burnout oven. The investment around the wax pattern is allowed to harden in air at
room temperature, and then it is heated to approximately 1200° F (650°C). At this temperature,
the investment and metal ring expand enough to compensate for the shrinkage of the gold alloy.
• When the investment has set, the layer at the top of the ring is trimmed off.
• The rubber crucible former is removed, and any loose particles of investment are blown off.
• The ring is then placed in the furnace for the recommended burnout schedule.
62
BURNOUT PROCEDURE
63
Burnout procedure
• Elimination of the wax pattern from the mould of set
investment material is referred to as the burnout.
• Ideally the casting ring containing the investment
should be placed into the oven approximately 1 hour
after investing the wax pattern.
• If the burnout procedure must be delayed for several
hours or overnight, it is advisable to place the
invested pattern into a humidor to prevent excessive
drying.
Investment rings should be placed in humidor to
prevent drying if it is anticipated that pattern will
not be burned out for several hours or overnight.
64
• To facilitate a rapid and clean burnout, the ring may
be placed on a raised object within the oven.
• A burnout started prematurely may cause fine cracks
in the gypsum-bonded investment.
• Once the heating is initiated, the casting should be
completed without permitting the mold to cool.
Porcelain tooth placed in bottom of oven provides good
support for one edge of ring, allowing molten wax and
gases to escape freely.
Cracks, caused by expanding steam, occur when damp investment
is heated too rapidly. This is major cause of fins on castings
65
• The mold should be placed in an oven preheated to approximately 900° F (480° C), held at
that temperature for 20 minutes, and the temperature then raised slowly to 1290° F (700° C)
and held for 30 minutes.
• Prolonged heating above 1290° F should be avoided.
• Gypsum-bonded investments will break down at this temperature, and the Sulphur and
chlorine will contaminate the gold alloy as it enters the mould.
• With a quartz investment, the rate of heating should be carefully controlled, since rapid
heating will produce a larger casting than will slow heating.
66
CASTING MACHINES
67
Classification Of Casting Machines
• Based on methods of casting the machines are:
1. Centrifugal force type
2. Air pressure type
3. Vacuum type
• Based on heating system employed:
1. Torch melted
2. Induction melted
3. Arc melted
68
Casting Machines
• Alloys are melted in one of the four following ways,
depending on the available types of casting machines:
1. The alloy is melted in a separate crucible by a torch
flame and cast into the mold by centrifugal force.
2. The alloy is melted electrically by a resistance heating
or induction furnace and then cast into the mold
centrifugally by motor or spring action.
Centrifugal casting machine, spring wound.
Spring-wound casting machine with electrical
resistance melting furnace.
69
3. The alloy is melted by induction heating and
then cast into the mold centrifugally by motor
or spring action.
4. The alloy is vacuum-arc melted and cast by
pressure in an argon atmosphere.
Induction melting casting machine with induction coil
Vacuum-arc Melting Machine
70
Torch Melting/Centrifugal Casting Machine
• The casting machine spring is first wound
from two to five turns.
• The alloy is melted by a torch flame in a
glazed ceramic crucible attached to the
“broken arm” of the casting machine.
• The broken arm feature accelerates the
initial rotational speed of the crucible and
casting ring, thus increasing the linear speed
of the liquid casting alloy as it moves into
and through the mold.
• Once the metal has reached the casting
temperature and the heated casting ring is in
position, the machine is released and the
spring triggers the rotational motion
71
Counter Weight
Tongs
Broken arm
Crucible former
Platform for
casting ring
Hinge for rotation
72
Zones of Flame
• Mixtures of natural gas and air, or oxyacetylene gases are used.
• Zone 1 - Non combustion zone/ Mixing Zone
• Zone 2 - Combustion zone
• Zone 3 - Reducing zone
• Zone 4 - oxidizing zone
73
Electrical Resistance–Heated Casting Machine
• In this device, current is passed through a resistance
heating conductor, and automatic melting of the alloy
occurs in a graphite or ceramic crucible.
• This is an advantage, especially for alloys such as those
used for metal-ceramic prosthesis, which are alloyed with
base metals in trace amounts that tend to oxidize on
overheating.
74
Induction Melting Machine
• With this unit, the alloy is melted by an induction
field that develops within a crucible surrounded by
water-cooled metal tubing.
• The electric induction furnace is a transformer in
which an alternating current flows through the
primary winding coil and generates a variable
magnetic field in the location of the alloy to be
melted in a crucible.
• Once the alloy reaches the casting temperature in
air or in vacuum, it is forced into the mold by
centrifugal force, air pressure, or vacuum. 75
Direct-Current Arc Melting Machine
• The direct-current arc is produced between two
electrodes: the alloy and the water-cooled tungsten
electrode.
• The temperature within the arc exceeds 4000 °C and
the alloy melts very quickly.
• This method poses a high risk of overheating the
alloy, and damage may result after only a few
seconds of prolonged heating.
76
Vacuum or Pressure-Assisted Casting Machine
• For this machine, the molten alloy is heated to the
casting temperature, drawn into the evacuated mold
by gravity or vacuum, and subjected to additional
pressure to force the alloy into the mould.
• For titanium and titanium alloys, vacuum arc heated-
argon pressure casting machines are required.
77
CASTING CRUCIBLE
78
Casting Crucible
• It is a vessel or container made of any refractory material (frequently ceramics) used for melting
or calcining any substance that requires a high degree of heat. (GPT- 9)
79
• Following are the types of crucible used for casting:
1. Clay crucible (for many of the crown and bridge alloys, such as
the high noble and noble types)
2. Carbon crucible (For high noble crown and bridge alloys but
also for the higher-fusing gold-based metal-ceramic alloys)
3. Quartz crucible (for high-fusing alloys of any type)
4. Ceramic crucible (For palladium-silver and nickel or cobalt
based alloys)
80
FLUX IN CASTING
81
Flux in casting
• A reducing flux should be used in melting the alloy.
• The flux (50% boric acid powder and 50% fused borax) increases the fluidity and reduces the
potential for oxidation.
• Flux maybe added to:
1. To minimizing porosity.
2. To increase fusing of metal.
3. Prevent oxidation.
82
HEAT TREATMENT
83
Heat Treatment
• To adequately resist excessive wear, restoration must be returned to a hardened state prior to its
clinical use.
• The physical properties, specifically the mechanical properties of some gold alloys, may be
modified by heat treatment.
• Gold alloys containing 7% or more copper will respond to heat treatment by changes in
microstructure, and consequently in their handling properties.
84
• Softening heat treatment consists of heating the alloy to 1290° F (700° C) and maintaining that
temperature for approximately 15 minutes, followed by quenching in room-temperature water.
• Hardening heat treatment may be conducted in either of two ways:
1. Heat soaking at a constant temperature of approximately 840° F (450° C) for 15 minutes
2. Low cooling from 840° to 480° F (450° to 250° C) over a period of 15 minutes, followed
by quenching in water.
85
CASTING PROCEDURES
86
Casting Procedures: Low-fusing Gold Alloys
• To melt low-fusing gold alloy for the casting procedure, three methods are available:
1. Compressed air and gas,
2. Oxygen and gas, or
3. An electric casting machine.
87
• When a torch is used flame cone should be
approximately 40 mm.
• The tip of the reducing cone is used to make a rapid
and clean melt.
• Electric furnace casting machine eliminates the need
for a torch and the judgment required in heating the
gold alloy. It is well controlled, accurate, and precise.
Properly adjusted torch.
(A) Reducing zone is used to melt gold. (B)Oxidizing
zone is cooler than reducing zone and will not heat
gold to proper casting temperature.
Electric casting machine
88
• If the investment cools prior to the casting, the mold
will become smaller through cooling contraction of
the investment.
• Castings produced with large amounts of alloy will
usually produce better detail and definition than
minimum amounts of metal used.
• If melted in a reducing flame, molten gold alloy that
has reached the proper temperature for casting will
appear shiny with a mirror like surface.
When gold has reached proper temperature for casting, it
will be elliptic with well-rounded edges, yellow-orange in
color, and will appear to be “spinning.”
89
• When the alloy has solidified and cooled for approximately 1 minute, the investment may be
placed into room-temperature water, and the alloy quenched.
• This will aid in removing the adhering investment, which can be cleaned from the casting with
a laboratory brush, toothbrush, or an air abrasive.
Pencil-type abrasive blasters can be used to remove
investment and oxides from casting without appreciable
danger of damaging margins.
90
Casting High-Fusing Metal-Ceramic Alloys
• Casting of porcelain-bonding alloys requires that the metal be heated approximately 212° F
(100° C) higher than its upper melting point.
• This is generally in the range of 2200° to 2500° F (1200° to 1370° C).
• These temperatures can be achieved with
1. A gas-oxygen torch or
2. By induction heating.
91
Induction Casting
• Induction casting can be used for alloys of any composition and provides for excellent control of
the casting temperature.
• The alloy is rapidly melted in a carbon crucible, heated by electrical induction.
• The atmosphere is reducing, and at casting the molten alloy temperature is centrifugally cast
into the mold.
• The apparatus for induction casting is expensive.
92
Torch Casting
• All alloys can be cast with a gas-oxygen or oxy-acetylene torch.
• The casting of porcelain-bonding alloys differs from casting low-fusing gold alloys in the
following respects:
1. No asbestos is used in the high-heat crucibles, since it may react with the alloy constituents at
high temperatures.
2. The technician should have one high-heat crucible for each brand of alloy being cast in order
to avoid cross-contamination.
3. No casting flux is used on porcelain-bonding alloys, since flux may alter its composition and
diminish the bond strength. This is particularly true of gold alloys.
4. The visual clues for assessing casting temperatures are different from low-fusing gold alloys,
since high-fusing alloys are heated white-hot before they are released into the mold.
93
5. Greater casting pressures (i.e., the number of turns of a centrifugal machine) are generally
required to force the porcelain-bonding alloy into the mold.
• When a multiple-sprue technique is used, the inlets should be aligned for the fastest and most
uniform distribution of alloy within the mold.
• The sprue and button should be sufficient to provide for cooling dynamics that do not lead to
shrinkage porosity.
94
• High-fusing gold alloys will melt into a pool that is cast
when it has reached a white-hot, almost vaporous state.
• Nonprecious nickel-chromium alloys are generally
supplied as sharp cornered ingots of various shapes and
are heated until the corners round over.
When gold alloy is ready to cast it will be white hot,
forming smooth oxide-free elliptical pool.
A, Base metal ingot— beginning of melt with gas-oxygen
flame.
B, Ingot continues to melt.
C, Base metal ingot ready to cast. Corners and sharp edges
have rounded.
D, Base metal ingot overheated, produces changes in
composition and excessive oxidation.
95
• All alloys should be melted as quickly as possible to
avoid excessive oxidation.
• High-fusing gold alloys are least sensitive to
overheating or prolonged heating.
• After casting, the machine should be allowed to spin
freely until it has nearly stopped .
• It may then be braked still, and the ring removed and
promptly quenched in water.
• The investment is initially removed by carving and
breaking it off the casting, taking care not to damage
the casting.
Investments must be carefully broken away from
casting. Attention to proper investing and casting
procedures will allow for clean separation of casting
from investment
96
Casting of Titanium alloys
• Advantages of titanium and titanium alloys include excellent
biocompatibility and corrosion resistance, which results from
the presence of a thin, adherent, passivating surface layer of
titanium dioxide.
• The dental casting of titanium and titanium alloys poses special
problems because of the high melting point of titanium
(1668°C) and its strong tendency to oxidize and react with other
materials.
• Titanium dental casting machines that represent a substantial
expense must provide either a vacuum environment or an argon
atmosphere.
• Both vacuum/argon pressure and centrifugal casting machines
have been developed, and both argon-arc melting and induction
melting have been used to fuse titanium and titanium alloys.
97
• Patterns for casting are coated, and investments must be used to provide the appropriate
expansion.
• Reaction of titanium or titanium alloy with the investment (and perhaps with the residual
atmosphere in the casting machine) results in a very hard near-surface region (termed α case)
that can exceed 50 μm in thickness.
• Currently, titanium castings of clinically acceptable accuracy can be produced, whereby the
marginal fit of cast complete crowns is superior to that for titanium crowns milled by the
computer-aided design/computer assisted manufacturing (CAD/CAM) technique.
98
CLEANING THE CASTING
99
Quenching
• After the casting has solidified, the ring is
removed and quenched in water as soon as the
button exhibits a dull-red glow.
• Two advantages are gained in quenching:
1. The noble metal alloy is left in an annealed
condition for burnishing, polishing, and similar
procedures, and
2. When the water contacts the hot investment, a
violent reaction ensues, resulting in a soft,
granular investment that is easily removed.
100
Pickling
• Often the surface of the casting appears dark with oxides and tarnish, such surface can be
removed by a process known as pickling.
• Pickling consists of heating the discolored casting in an acid.
• One of the best pickling solutions for gypsum-bonded investments is a 50% hydrochloric
acid solution.
• Nonprecious nickel-chromium alloys must never be placed in acid because of their high
reactivity.
• The hydrochloric acid aids in the removal of any residual investment, as well as of the oxide
coating.
101
• 'The best method for pickling is to place the casting in a test tube or dish and to pour the acid
over.
• The pickling solution should be renewed frequently, because it is likely to become contaminated
after reusing the solution several times.
• In no case should the casting be held with steel tongs so that both the casting and the tongs come
into contact with the pickling solution, because this may contaminate the casting.
• When the steel tongs contact electrolyte, a small galvanic cell is created and copper is deposited
on the casting at the point where the tongs grip it which becomes future source for discoloration
in the area.
102
Sandblasting
• The process of altering the surface of a material through the use of abrasive particles
propelled by compressed air or other gases. (GPT-9).
• It can be done using a high speed sandblaster.
• Most common medium for sandblasting in dentistry is aluminum oxide.
• The fine aluminum oxides are recycled within the sandblasting machine and replaced after
30- 40 minutes of total accumulated operation time.
• 60-80 psi of force is exerted by the machine.
103
• Provides mechanical retention between porcelain-metal by removing the casting oxides as well
as proper sandblasting of the alloy with 100-150 microns aluminum oxide results to mechanical
bonding.
• Also provides micromechanical retention of denture base to framework.
• Two types of sandblasting
1. Automatic sandblaster
2. Blast cabinets
104
Cleaning The Casting
• The first step is to thoroughly clean the surfaces of all
residual investment.
• Abrasive blasting is effective for this.
• The blasting medium can become embedded in the
surface and be a source of contamination if not
thoroughly removed.
• Traces of investment can easily be ground into the
metal surface and act as sources of gas at the
porcelain -metal interface when porcelain is added.
Residual investment
(I) is easily removed from casting
(C) by use of Al203 or glass bead powders in pencil-
tip air-abrasive units. Margins are easily protected by
using this type apparatus .
105
• Resin-bound abrasives (e.g., some carborundum or paper
disks) can contaminate the metal surface with resin,
leading to severe bubbling when porcelain is added.
• Once the porcelain-bearing surface is clean, it may
optionally be sandblasted with a clean 25 to 50 µm
aluminum oxide abrasive to texturize it.
Contamination of metal surface by finishing with
resin bound abrasives can lead to severe bubbling
in porcelain. This layer must be removed with
hydrofluoric acid and metal refinished with no
contaminating, ceramic-bound abrasives.
106
• This will increase the area of bonding and improve
the wettability of the metal.
• Surface roughness is not necessary to achieve a
satisfactory porcelain-to-metal bond, since the main
mode of attachment is chemical, not mechanical
• The casting can now be cleaned in distilled water in
an ultrasonic cleaner.
• When the metal surface is absolutely clean — free of
oxides, investment and organic films — it is ready for
the next stage of metal conditioning (finishing).
Aluminum oxide air- abrasion of metal surface after
finishing with ceramic -bound stones will produce uniform
texture and improve wettability by opaque porcelain.
107
FINISHING OF CASTING
108
Objectives And Procedures
• The objectives and procedures for finishing
are different for each part of the cast
restoration.
• Zone 1 is the internal margin
• Zone 2 the internal surface
• Zone 3 the sprue
• Zone 4 the proximal contacts
• Zone 5 the occlusal surface
• Zone 6 the axial walls and
• Zone 7 the external margins.
109
Zone 1: Internal Margin
Objective:
• To minimize any dissolution of the luting agent, a 1-
mm wide band of metal must be closely adapted to
the tooth surface.
• A discrepancy within this zone can significantly
reduce a restoration’s longevity.
• Good adaptation is obtained by careful reflowing of
the wax pattern.
Reflowing of the wax pattern. The objective is to create a
well-adapted 1-mm zone to prevent cement dissolution.
Proper reflowing before investing is essential.
110
Procedure for Zone-1
• If a defect occurs in the marginal area, the restoration must be remade.
• Even small nodules can prevent a casting from seating completely.
• Small nodules, if far enough away from the margin itself, can be removed under a binocular
microscope with exceptionally cautious use of small rotary instruments (e.g., a No. 1/2 round
bur).
111
Zone 2: Internal Surface (Intaglio)
Objective:
• No contact should exist between the die and the internal surface (intaglio) of the casting.
• A uniform space of 25 to 35 μm is necessary for the luting agent to spread evenly.
• Any contacts must be identified and relieved by careful selective grinding of the internal
surface.
112
Procedure for Zone-2
• Casting’s internal surface should, be examined for nodules
before the restoration is seated on the die.
• Even a very small nodule can result in significant increase of the
marginal gap width.
• Any significant force will abrade or chip the die, so that the
casting will seat on the die but will not seat fully on the prepared
tooth.
113
• Once the casting has been adjusted, determining
the exact location of the nodule is no longer
possible.
• Therefore, the nodule should be removed
entirely in one step, rather than through
sequential relief of the internal surface.
• Several agents are commercially available to
facilitate identification of the seating interference
between the casting and the die. When a nodule is removed, removal of slightly more than the
defect ensures complete seating of the restoration.
114
A, Incomplete seating.
B, Liquid marking agent.
C, A thin coat is applied to the internal surface and air dried.
D, The casting is gently returned to the die.
E, The area of interference is identified.
F, Nodules are best removed with a small round bur.
G, Seated casting.
A B C D
EFG
115
Zone 3: The Sprue
Objective
• To re-establish proper coronal structure and function, the sprue must be sectioned, and the
casting must be recontoured in the area of its attachment.
Procedure for Zone- 3:
• Once the fit of the casting has been verified on the die and it has been found to be acceptable,
the sprue is sectioned, and the area of its attachment to the casting is reshaped.
116
(A)Attached sprue to casting
(B)cut around the sprue and then twist it off.
(C)With multiple castings made simultaneously, care
must be taken not to damage the margin inadvertently.
(D)Disks and stones are used for gross recontouring.
B
C
A
D
117
Zone 4: Proximal Contacts
Objective
• The proximal contact areas are adjusted in the laboratory so that they will be correct (or slightly
too tight) when the casting is evaluated in the patient’s mouth.
118
Procedure for Zone-4
• The proximal contacts on the stone cast can be minimally
relieved by careful scraping with a scalpel.
• When proximal contacts are adjusted, placing a thin
articulating film between adjacent castings or between the
casting and the adjacent tooth is helpful.
• Doing this allows the areas where binding contact occurs
to be adjusted through selective adjustment where
markings result.
119
A, Thin articulating film interposed between a metal-ceramic restoration and the adjacent tooth.
B, The area of contact that prevents complete seating is readily apparent.
C, Articulating film is used to detect the location of an excessive proximal contact on cast metal.
A B C
120
Zone 5: Occlusal Surface
Objective
• Occlusal contacts are re-established in static and dynamic relationships to the opposing arch.
• Obtaining accurate and stable contacts does not require highly polished metal occlusal surfaces;
a satin finish is acceptable.
• Occlusal form must ensure positional stability and satisfy all functional requirements.
121
Procedure for Zone-5
• The occlusal contacts are checked with thin articulating film to
ensure that they match the design in the waxing stage.
• If an occlusal contact is heavy in wax, it springs back slightly
when the articulator is opened and produces an occlusal
prematurity in the casting.
A and B, Occlusal prematurity's are
generally the result of excessively heavy
contact on the wax pattern.
B
A
122
• Occlusal adjustments can be performed with flame shaped
finishing burs or diamond bur.
• The correct technique for occlusal adjustment is to re-develop the
anatomy of the entire ridge or cusp rather than grinding only the
point of interference.
• Simultaneously, any nodules can be removed, and grooves can be
defined with a finishing bur or a small round bur.
A, Occlusal adjustment is readily accomplished
with a pointed diamond or carbide bur.
B, The grooves and fissures are concurrently
refined.
B
A
123
• Before starting any adjustment, the practitioner should
use a thickness gauge on the metal.
• If only minimum clearance was established at the tooth
preparation stage, indiscriminate adjustment leads to
inadequate thickness of the casting.
As occlusal adjustments are made
(A), the residual thickness is continually monitored with an
appropriately designed thickness gauge
(B). For structural durability, metal thickness of less than
1.0 mm is inadequate and is the result of insufficient
occlusal reduction.
124
• If the wax pattern has been carefully
finished, a smooth casting results, and
removing surface oxides with a soft wire
brush wheel is sufficient.
• The surface can then be polished with
rouge on a soft brush wheel (which
removes only 5 μm from the surface of
the casting.
A, Initially a wire brush is used on the occlusal surfaces.
B, A fine-grit sandpaper disk is applied for removing pits and irregularities from the axial walls
C A rubber wheel is then used on the axial walls.
D, Castings, after polishing with buffing compound, immediately before clinical evaluation.
E The completed castings immediately before cementationE
DC
BA
125
Zone 6: Axial Walls
Objective
• When axial wall finishing is completed, the walls should be smoothly contoured and highly
polished, enabling the patient to perform optimum plaque control.
126
Procedure for Zone-6
• Surface defects are removed by grinding with
abrasive particles bound into a grinding stone
or rubber wheel, on a paper disk, or applied
as an abrasive paste.
• A sequence of progressively finer grades is
used to attain the desired surface.
(A)Carborundum disks and stones of varying degrees of coarseness are
typically used first;
(B)these are followed by garnet paper and sandpaper disks,
(C)rubber points and white Arkansas stones,
(D)and rubber wheels and points, along with small carbide burs for
removing nodules.
C
B
D
A
127
• The most efficient method of polishing
is to use a sequence of progressively
finer abrasives each removing the
scratches made by the previous grade.
• Time is wasted if the progression to a
finer grade abrasive is too rapid
because the coarser grits remove
material much more efficiently.
A, Assorted abrasives, sandpaper disks, rubber points, and polishing wheels.
B, Instruments used range from small carbides (for removing nodules) and a steel wire brush (for occlusal surface
smoothing) to buffing wheels and compounds.
C, A coarse wheel is used to true and thin the edge of a rubber wheel.
D, Buffing compounds applied on a wheel or bristle brush.
A
D
B
C
128
Zone 7: External Margins
Objective
• Margin finishing is crucial for a restoration’s longevity and therefore merits special attention.
• The objective of all cast restoration finishing is a highly polished metal surface without ledges
or steps as the transition is made from restoration to unprepared tooth.
• Failure to accomplish this leads to compromised plaque control.
129
Procedure for Zone-7
• Where access allows, cavo-surface margins
should be finished directly on the tooth.
A Supragingival margins allow access for finishing the
restoration directly on the tooth.
B, Fine-grit white stone lubricated with petroleum jelly.
C, Rubber point.
D, Completed restoration.
A
C D
B
130
A. When subgingival margins do not allow access, final finishing is performed on the die. During final
polishing, the margin is carefully supported with a finger.
B. Carefully rubbing a smooth instrument along the length of the margin (burnishing).
C. Gently brushing a fine-grit stone over the surface to remove casting roughness Using a soft rubber
wheel or point.
CBA
131
DEGASSING CERAMOMETAL
CASTINGS
132
Degassing Ceramometal Castings
• After the coping or framework is cleaned, it should be subjected to a degassing or surface –
conditioning treatment.
• During degassing the unit is heat treated to remove contaminants from the surface or possibly to
remove entrapped gas from the alloy .
• In addition, a thin oxide film is formed on the surface. This film is essential to porcelain
bonding.
• Precious gold alloys should be rapidly heated in air to 1950° F (1065° C ), held there 5 to 10
minutes , and rapidly cooled to room temperature.
133
• The unit will have darkened due to surface oxidation .
• Semiprecious and base metal alloys are generally heated to 1950° F , and held at this
temperature in a 25- to 28- inch (64- to 70- cm) mercury vacuum for 5 to 10 minutes.
• At this temperature the vacuum can be broken and the unit then cooled quickly. This procedure
will produce a thin but sufficient oxide coating on the metal surface.
• A second aluminium oxide (Al2O3) abrasive blasting of the surface is recommended for base
metal alloys to remove excessive oxidation.
134
CASTING DEFECTS
135
Casting Defects
• Defects in castings can be classified under four headings:
1. Distortion;
2. Surface roughness and irregularities;
3. Porosity and
4. Incomplete or missing detail
136
Distortion
• Distortion of the casting is probably related to a
distortion of the wax pattern, it can be minimized by
proper manipulation of the wax and handling of the
pattern.
• The setting and hygroscopic expansions of the
investment may produce a non-uniform expansion of
the walls of the pattern.
• Factors that affect distortion are:
1. The configuration of the pattern,
2. The type of wax, and
3. The thickness influence the distortion that occurs
• Distortion increases as the thickness of the pattern
decreases, the lower is the setting expansion of the
investment, the less lower is distortion.
137
Surface Roughness, Irregularities,
And Discoloration
• Surface roughness is defined as relatively finely spaced surface
imperfections whose height, width, and direction establish the
predominant surface pattern.
• Surface irregularities are isolated imperfections, such as nodules,
that are not characteristic of the entire surface area.
• Improper technique can lead to a marked increase in surface
roughness as well as to the formation of surface irregularities.
138
• Surface discoloration and roughness can result from
sulfur contamination.
• The interaction of the molten alloy with sulfur produces
a black or gray layer on the surface of gold alloys that is
brittle and does not clean readily during pickling.
A black-coated noble metal alloy casting resulting from
sulfur contamination or oxidation during melting of the
alloy.
139
Air Voids
• Small nodules on a casting are caused by air
bubbles that become attached to the pattern during
or subsequent to the investing procedure.
• The best method to avoid air bubbles is to use the
vacuum investing technique.
• A wetting agent may be helpful in preventing the
collection of air bubbles on the surface of the
pattern.
• It is best to air-dry the wetting agent, because any
excess liquid dilutes the investment, possibly
producing surface irregularities on the casting.
140
Water Films
• Wax is repellent to water; if the investment becomes
separated from the wax pattern in some manner, a
water film may form irregularly over the surface.
• If the pattern is slightly moved, jarred, or vibrated
after investing or if the painting procedure does not
result in intimate contact of the investment with the
pattern, such a condition may result.
• If too little water is used, the investment may be un-
manageably thick, so that it cannot be properly
applied to the pattern.
• A wetting agent is useful for the prevention of such
irregularities. 141
Foreign Bodies
• When foreign substances get into the mold a surface
roughness may be produced
• A rough crucible former with investment clinging to it may
roughen the investment on its removal so that bits of
investment are carried into the mold with the molten alloy.
• Usually contamination results not only in surface roughness
but also in incomplete areas or surface voids.
• Any casting that shows sharp, well-defined deficiencies
indicates the presence of some foreign particles in the mold,
such as pieces of investment and bits of carbon from a flux.
• Bright-appearing concavities may be the result of flux being
carried into the mould with the metal.
142
Impact Of Molten Alloy On The Mold Wall
• The direction of the sprue former should be such that the molten gold alloy does not impact a
weak portion of the mould surface.
• Sometimes the abraded area is smooth, so that it cannot be detected on the surface of the
casting.
• Such a depression in the mould is reflected as a raised area on the casting, which prevents
complete seating of the casting.
• It can be avoided by proper spruing so as to prevent the direct impact of the molten metal at an
angle of 90° to the investment surface.
143
Pattern Position
• If several patterns are invested in the same ring, they should not be placed too close together.
• Likewise, positioning too many patterns in the same plane in the mould should be avoided.
• The expansion of wax is much greater than that of the investment, and this may cause
breakdown or cracking of the investment if the spacing between patterns is less than 3 mm.
144
Carbon Inclusions
• Carbon from a crucible, an improperly adjusted torch, or a carbon-containing investment, can be
absorbed by the alloy during casting.
• These particles may lead to the formation of carbides or even create visible carbon inclusions.
145
Porosity
• Porosity may occur both within the interior region of a casting and in the external surface which
results in surface roughness.
• Internal porosity weakens the casting and also cause discoloration.
• If severe, it can cause plaque accumulation at the tooth-restoration interface, and secondary
caries or periodontal disease may result within the adjacent tooth structure.
• Although porosity in a casting cannot be prevented entirely, it can be minimized by the use of
proper techniques.
146
Porosities in noble metal alloy castings are classified below.
• Solidification defects
A. Localized shrinkage porosity
B. Microporosity
C. Suck-back porosity
• Trapped gases
A. Pinhole porosity
B. Gas inclusions
C. Subsurface porosity
D. Back pressure porosity
147
Localized Shrinkage
• Generally caused by premature termination of the flow of
molten metal during solidification.
• Continual feeding of molten metal through the sprue must
occur to make up for the shrinkage of metal volume during
solidification.
• Localized shrinkage generally occurs near the sprue-casting
junction.
• If the sprue freezes in its cross section before this flow is
completed, a localized shrinkage void will occur in the last
portion of the casting that solidifies.
Localized shrinkage porosity in pontic of
three-unit bridge caused by delayed
solidification and lack of a chill-set sprue.
148
Microporosity
• Microporosity occurs from solidification shrinkage.
• It occurs when the solidification is too rapid for the micro-voids
to segregate to the liquid pool.
• This premature solidification causes the formation of small,
irregular voids.
• Such phenomena can occur from rapid solidification if the mold
or casting temperature is too low.
149
Pinhole- Porosity
• Oxygen is dissolved by some of the metals, while they are in the
molten state.
• During solidification, the gas is expelled to form blebs and pores
in the metal.
• The porosity that extends to the surface is usually in the form of
small pinpoint holes.
• When the surface is polished, other pinholes appear.
150
Gas Inclusion Porosity
• The gas inclusion porosities are usually much larger than pinhole porosity.
• Larger spherical porosities can be caused by gas occluded from a poorly adjusted torch flame or
by use of the mixing or oxidizing zones of the flame rather than the reducing zone.
• If the alloy has been used before, these types of porosities can be minimized by pre-melting and
correctly adjusting and positioning the torch flame during melting.
151
Subsurface Porosity
• They may be caused by the simultaneous nucleation of solid grains
and gas bubbles at the first moment that the alloy freezes at the
mould walls.
• This type of porosity can be diminished by controlling the rate at
which the molten metal enters the mould.
152
Suck-Back Porosity
• It occurs externally, usually in the interior of a crown near the area
of the sprue, if a hot spot has been created by the hot metal
impinging from the sprue channel on a point of the mould wall.
• The entering metal impinges onto the mold surface at this point
and creates a higher localized mold temperature in this region,
known as a hot spot.
• This hot spot causes the local region to freeze last and results in
what is called suck-back porosity.
• Suck-back porosity often occurs at an occluso-axial line angle or
inciso-axial line angle that is not well rounded.
153
• A hot spot may retain a localized pool of molten metal after other
areas of the casting have solidified.
• This, in turn, creates a shrinkage void or suck back porosity.
• This type of porosity defect can be eliminated by flaring the point
of sprue attachment and reducing the mold-melt temperature
differential—that is, lowering the casting temperature by about
30 °C.
154
Back-Pressure Porosity
• Entrapped air bubbles on the inner surface of the casting, are
sometimes referred to as back-pressure porosity.
• This is caused by the inability of the air in the mold to escape
through the pores in the investment or by the pressure gradient
that displaces the air pocket toward the end of the investment
via the molten sprue and button.
• Frequently found at the cavity surface of a crown or mesio-
occlusal-distal casting.
• It can be prevented by use of the dense modern investments,
by an increase in mold density produced by vacuum investing,
and by the tendency for the mold to clog with residual carbon
when the low-heat technique is used.
155
Incomplete Casting
• The obvious cause is that the molten alloy has been prevented in some
manner from completely filling the mould.
• At least two factors that may inhibit the ingress of the liquefied alloy
are insufficient venting of the mold and high viscosity of the fused
metal.
• The first consideration, insufficient venting, is directly related to the
back pressure exerted by the air in the mould.
• If the air cannot be vented quickly, the molten alloy does not fill the
mold before it solidifies.
• These failures are usually exemplified by rounded, incomplete
margins. 156
• A second common cause of an incomplete casting is
incomplete elimination of wax residues from the mold.
• If too many products of combustion remain in the mold, the
pores in the investment may become filled, so that the air
cannot be vented completely.
Incomplete casting resulting from incomplete wax
elimination is characterized by rounded margins and
shiny appearance.
157
SUMMARY OF CASTING
DEFECTS
158
Type of Failure Procedural Errors Solution
Suck-back porosity Sprue attached at a right angle to
the wax pattern, creating a
“hot spot”
Sprue should always be attached at
the bulkiest portion of the wax pattern
directed at 45° to the surface
Improper margin fit Improper handling of wax pattern
during removal from the oral
cavity
Hard wax can be used for wax pattern
fabrication.
Careful handling of the pattern during
removal along the path of insertion,
taking care not to disturb the margins
Air bubble in the
Casting
Air bubble entrapment during
investing procedure
Prevented by carrying out the mixing
and investing procedure under
vacuum
159
Type of Failure Procedural Errors Solution
Water film Pattern is slightly moved, jarred, or
vibrated after investing
Prevented by proper use of a wetting
agent and proper care of the invested
casting ring
Contamination of the alloy Reaction of the alloy with crucible
used
Crucible unable to withstand the
temperature
Choose appropriate crucible for each
alloy
Microporosities Solidification occurs too rapidly
(when the mold or casting
temperature is too low)
Proper temperature to be maintained
160
Type of Failure Procedural Errors Solution
Pits in casting • Debris in mould
• Dirty wax
• Loose debris in crucible
• Mould temperature too hot
• Join ingate, sprue former, and
pattern with continuous smooth
surface with no jagged areas of
investment to be broken off and
pushed into mold ahead of alloy
• Use only clean, new wax for
patterns and sprue formers
• Use clean crucible for each casting
• Lower burnout temperature since
too high temperature causes
investment breakdown, producing
weak surface easily abraded by
alloy
Fins on castings • Over vibration during investment
or disturbing ring during set
• Heating ring too rapidly causes
moisture in mold to form steam
and rupture out mold
• Avoid over vibration and place
investment ring in area free from
disturbances until investment is
completely set
• Heat mold slowly.
161
Type of Failure Procedural Errors Solution
Localized shrinkage porosity &
Incomplete casting
• Using a sprue with a very small
diameter
• Discrepancy in temperatures
between the casting ring/ mold and
the molten alloy
• Insufficient casting pressure during
the casting process
• Incomplete elimination of wax and
incomplete venting
• Higher viscosity of the molten alloy
Larger sprue diameter to allow proper
flow of molten metal into the mold
• Sprue to be attached at the bulkiest
portion of the wax pattern directed at
45° to the surface
• Proper balance between mold and
molten alloy temperatures
• Pressure on the arm of the casting
machine should be maintained for at
least 4 sec to allow the alloy to fill the
mould
• A vent of 0.5 mm in diameter should
be provided to allow escape of gases
• Proper casting temperature of the
molten metal to be maintained during
casting
Contamination of the casting The casting held with steel tongs
during pickling
Use of steel tongs should be avoided
162
Type of Failure Procedural Errors Solution
Rounded margins • Incomplete burnout of wax
pattern
• Insufficient heating of alloy
before casting
• Margins melted while
attaching pattern to sprue or
former
• Improper diameter/length of
sprue restricts flow of alloy
into mold; metal freezes
before margins are complete
• Heat soak mould for 1 hour
at minimum of 950° F (510°
C) to ensure elimination of
carbon residue
• Heat alloy to 150° F (57° C)
above fusion temperature at
moment of casting alloy
• Keep pattern and sprue
former in horizontal position
when attaching, so that heat
rising from instrument does
not soften pattern
• Average casting should have
10-gauge sprue
approximately 6 mm long
163
Type of Failure Procedural Errors Solution
Rough surface on casting • Excess moisture on pattern
• Water-powder ratio too high
in mixing investment
• Too much casting pressure,
causing investment
breakdown from force of
alloy
• Prolonged overheating of
gypsum- bound investment
• Remove all moisture from
pattern, sprue former, and
ring
• Use correct water-powder
ratio
• Do not wind machine too
tightly
• Use correct heating cycle for
burnout procedure; do not
heat above 1290° F (700° C)
164
REVIEW OF LITERATURE
165
Lombardas P, Carbunaru A, McAlarney ME, Toothaker RW, of Dental S, Oral
Surgery NY. Dimensional accuracy of castings produced with ringless and
metal ring investment systems. The Journal of prosthetic dentistry. 2010 Jul
1;84(1):27 31.
• Lombardas et al did a study to determine “Dimensional accuracy of castings produced with
ringless and metal ring investment systems”
• This study compared the vertical margin accuracy of lost wax castings produced with the
conventional casting technique using a metal ring and a technique that uses a ringless system.
• From copings fabricated on a metal die,
1. 30 castings were produced from a high palladium alloy for metal ceramic restorations
2. 10 castings were cast with phosphate-bonded investment with the ringless technique
3. 10 were cast with the phosphate-bonded investment with a metal ring, and
4. The final 10 were cast using Hi-temp (Whip Mix) phosphate-bonded investment with a metal
ring.
166
• The internal surface of the castings were not modified before seating with finger pressure. For
vertical margin discrepancy measurements, an optical microscope at a magnification of 100×
was used. Data were analyzed with 1-way ANOVA (repeated measures) and the Student test.
• When following the manufacturers’ recommendations, the castings of the ringless technique
provided less vertical margin discrepancy (mean value 181 ± 71 μm) than the castings produced
with the conventional metal ring technique (290 ± 87 μm and 291 ± 88 μm). The difference was
significant (P<.001)
167
• Within the conditions of this study, the following conclusions were drawn:
1. The vertical margin discrepancy of the ringless group for the buccal, the lingual, and the distal
sites were significantly less than that of the 2 ring groups (P<.001).
2. There was no significant difference of the vertical margin discrepancy between the 2 metal
ring groups.
3. There was no significant difference in the vertical margin discrepancy at the buccal, lingual,
mesial, and distal surfaces within the same group.
4. The ringless technique was clinically acceptable and can be used for the fabrication of fixed
prosthodontic restorations.
168
Prabhu KG, Eswaran MA, Phanikrishna G, Deepthi B. Sprue design
alterations and its effect on the properties of base metal alloy castings: An in
vitro study. Journal of pharmacy & bioallied sciences. 2015 Aug;7(Suppl
2):S524.
• Prabhu et al did a study on to evaluate “Sprue design alterations and its effect on the properties
of base metal alloy castings: An in vitro study.”
• To study the effect of various sprue designs on the properties of base metal alloy castings. The
base metal alloys are extensively used for their excellent properties such as an increase in
hardness, high melting range, high elastic modulus, its compatibility with ceramic material and
low cost.
• However, to improve the properties of the base metal alloys is leading to various modifications
in their fabrication procedure – which include sprue designs and their mode of attachment to the
wax pattern.
169
• Study compared the effect of three sprue designs on the properties of mass and micro-hardness
of base metal alloy castings. viz.
1. Conical sprue,
2. Cylindrical sprue and
3. Bottleneck sprue
• A prefabricated wax mesh pattern was selected for the fabrication of the alloy test samples in the
study.
• The cylindrical sprue design was connected to the mesh pattern with a straight attachment.
• The bottleneck sprue design was connected to the mesh pattern with a constricted attachment.
• The conical sprue design was connected to the mesh pattern with a flared attachment.
• In this manner, ten samples for each of the three different sprue designs were prepared.
170
• Results: The obtained value for mass and microhardness were subjected to statistical analysis.
ANOVA test was performed to determine the difference between the sprue designs.
• Conclusion: The bottleneck sprue, conical sprue, and cylindrical sprue designs did not exert any
apparent influence on the mass and microhardness.
171
Earnshaw R. The effect of casting ring liners on the potential expansion of a
gypsum-bonded investment. Journal of dental research. 2010 Nov;67(11):1366-
70.
• Earnshaw R. did a study to determine “The effect of casting ring liners on the potential
expansion of a gypsum-bonded investment”
• A study was conducted on cellulose paper, ceramic paper and asbestos paper of the effects on
the setting and subsequent thermal expansion of a gypsum-bonded cristobalite casting
investment.
• Thermal expansion measurements were made on the same specimens that were produced during
the setting expansion tests.
• Control specimens setting against a smooth dry surface showed a total expansion of 1. 7%.
Specimens setting against dry ceramic liners had similar total expansions, in the range 1. 6 to 1.
7%.
• Specimens setting against either of the wet lining materials showed an increased total expansion
(in the range 2.2 to 2.3%), by virtue mainly of a large increase in setting expansion.
172
• Dry asbestos and dry cellulose liners gave higher expansions than pre-wetted ones, since they
abstracted water from the mix, reducing its effective W/P ratio (giving a thicker mix), and then
functioned as wet liners.
• These results suggest that, at least as far as potential investment expansion is concerned, wet
cellulose liners have an effect similar to that of the traditional wet asbestos liners.
• Dry ceramic liners give a much lower investment expansion, and when these liners are used, an
investment with an increased measured expansion could be an advantage.
173
Baskaran BE, Prabhu KG, Prabhu R, Krishna GP, Eswaran MA, Gajapathi B.
Casting made simple using modified sprue design: An in vitro study. Indian
Journal of Dental Research. 2014 May 1;25(3):340.
• Baskaran et al did a study on “Casting made simple using modified sprue design: An in vitro
study”.
• Regardless of the alloy used for casting, the casting technique should yield a casted alloy, which
should possess sufficient mass, surface hardness and minimal porosity after casting.
• Twenty patterns for casting were made from three-dimensional printed resin pattern simulating a
3 unit FPD and casted using modified sprue technique.
• Later test samples were cemented sequentially on stainless steel model using pressure indicating
paste and evaluated for vertical marginal gap in eight predetermined reference areas.
174
• Marginal gap were measured in microns using Video Measuring System. A portion of the axial
wall of the cast abutments depicting premolar and molar were sectioned and embedded in
acrylic resin and tested for micro hardness and porosity.
• The results obtained for marginal gap, micro hardness, and porosity of all test samples were
tabulated, descriptive statistics were calculated and the values were found to be within the
clinically acceptable range.
• Thus new sprue technique can be an alternative and convenient method for casting which would
minimize metal wasting and less time consuming.
175
REFERENCES
• Kenneth J. Anusavice. Philip’s Science of Dental Material. 11th Edition. St. Louis, Missouri:
Saunders Elsevier; 2003.
• Rosenstiel, Land, Fujimoto. Contemporary Fixed Prosthodontics. 5th Edition. St. Louis
Missouri: Saunders Elsevier; 2016.
• Herbert T Shillingburg, David Sather, Joseph Cain, Luis Blanco. Fundamentals of Fixed
Prosthodontics. 4th Edition. Hanover Park, Illinois, USA: Quintessence Publishing Co, Inc;
2012.
• Robert Marrow, Kenneth Rudd, John Rhoads. Dental Laboratory Procedures Volume II. 2nd
Edition. St. Louis, Missouri: Mosby; 1986
• V Shama Bhat, Nandish BT. Science of Dental Materials. 2nd Edition. Delhi: CBS Publishers;
2013
• S Mahalaxmi. Materials used in dentistry. 1st Edition. Haryana: Wolters Kluwer Health; 2013
176
• Robert Marrow, Kenneth Rudd, John Rhoads. Dental Laboratory Procedures Volume III. 2nd
Edition. St. Louis, Missouri: Mosby; 1986
• Lombardas P, Carbunaru A, McAlarney ME, Toothaker RW, of Dental S, Oral Surgery NY.
Dimensional accuracy of castings produced with ringless and metal ring investment systems.
The Journal of prosthetic dentistry. 2010 Jul 1;84(1):27 31.
• Earnshaw R. The effect of casting ring liners on the potential expansion of a gypsum-bonded
investment. Journal of dental research. 2010 Nov;67(11):1366-70.
• Prabhu KG, Eswaran MA, Phanikrishna G, Deepthi B. Sprue design alterations and its effect on
the properties of base metal alloy castings: An in vitro study. Journal of pharmacy & bioallied
sciences. 2015 Aug;7(Suppl 2):S524.
• Baskaran BE, Prabhu KG, Prabhu R, Krishna GP, Eswaran MA, Gajapathi B. Casting made
simple using modified sprue design: An in vitro study. Indian Journal of Dental Research. 2014
May 1;25(3):340.
177
THANK YOU
178

More Related Content

What's hot

Cavity liners and_bases_2
Cavity liners and_bases_2Cavity liners and_bases_2
Cavity liners and_bases_2
Dinesh Khatri
 

What's hot (20)

Inlay
InlayInlay
Inlay
 
Investment materials
Investment materialsInvestment materials
Investment materials
 
Cavity liners and_bases_2
Cavity liners and_bases_2Cavity liners and_bases_2
Cavity liners and_bases_2
 
CASTING PROCEDURES AND DEFECTS
CASTING PROCEDURES AND DEFECTSCASTING PROCEDURES AND DEFECTS
CASTING PROCEDURES AND DEFECTS
 
Investment materials
Investment materialsInvestment materials
Investment materials
 
Casting in dentistry
Casting in dentistryCasting in dentistry
Casting in dentistry
 
Dental+ceramics
Dental+ceramicsDental+ceramics
Dental+ceramics
 
Burs in dentisty ashish
Burs in dentisty ashishBurs in dentisty ashish
Burs in dentisty ashish
 
Composite resin technique
Composite resin techniqueComposite resin technique
Composite resin technique
 
Dental waxs
Dental waxsDental waxs
Dental waxs
 
Dental Casting alloy
Dental Casting alloyDental Casting alloy
Dental Casting alloy
 
Casting defects
Casting defectsCasting defects
Casting defects
 
Class II Inlay
Class II InlayClass II Inlay
Class II Inlay
 
Casting procedures in dentistry
Casting procedures in dentistryCasting procedures in dentistry
Casting procedures in dentistry
 
Class II cavity preparation
Class II cavity preparationClass II cavity preparation
Class II cavity preparation
 
Soldering & welding
Soldering & weldingSoldering & welding
Soldering & welding
 
GIC
GICGIC
GIC
 
Dental casting alloys
Dental casting alloysDental casting alloys
Dental casting alloys
 
Tissue-conditioners
Tissue-conditionersTissue-conditioners
Tissue-conditioners
 
Recent Advances in Dental Ceramics
Recent Advances in Dental CeramicsRecent Advances in Dental Ceramics
Recent Advances in Dental Ceramics
 

Similar to Casting Procedures & Casting Defects in Dentistry

The Manufacturing Processes - Foundary.pdf
The Manufacturing Processes - Foundary.pdfThe Manufacturing Processes - Foundary.pdf
The Manufacturing Processes - Foundary.pdf
pgarg210405
 

Similar to Casting Procedures & Casting Defects in Dentistry (20)

casting defects
casting defectscasting defects
casting defects
 
Cast
CastCast
Cast
 
Casting procedures
Casting procedures Casting procedures
Casting procedures
 
Casting procedure
Casting procedure Casting procedure
Casting procedure
 
Mould gating system for foundry and metal casting
Mould gating system for foundry and metal castingMould gating system for foundry and metal casting
Mould gating system for foundry and metal casting
 
Gating system :- CASTING PROCESSES
Gating system :- CASTING PROCESSESGating system :- CASTING PROCESSES
Gating system :- CASTING PROCESSES
 
Casting procedure & casting defects
Casting procedure & casting defectsCasting procedure & casting defects
Casting procedure & casting defects
 
Casting procedures and defects/prosthodontic courses
Casting procedures and defects/prosthodontic coursesCasting procedures and defects/prosthodontic courses
Casting procedures and defects/prosthodontic courses
 
CASTING DEFECT.pptx
CASTING DEFECT.pptxCASTING DEFECT.pptx
CASTING DEFECT.pptx
 
Casting procedures
Casting proceduresCasting procedures
Casting procedures
 
Casting procedures & defects
Casting procedures & defectsCasting procedures & defects
Casting procedures & defects
 
Manufacturing Technology of Materials in Engineering
Manufacturing Technology of Materials in EngineeringManufacturing Technology of Materials in Engineering
Manufacturing Technology of Materials in Engineering
 
Final project ppt
Final project pptFinal project ppt
Final project ppt
 
The Manufacturing Processes - Foundary.pdf
The Manufacturing Processes - Foundary.pdfThe Manufacturing Processes - Foundary.pdf
The Manufacturing Processes - Foundary.pdf
 
casting in manufacturing process in me.pptx
casting in manufacturing process in me.pptxcasting in manufacturing process in me.pptx
casting in manufacturing process in me.pptx
 
LAB PROCEDURES IN CPD
LAB PROCEDURES IN CPDLAB PROCEDURES IN CPD
LAB PROCEDURES IN CPD
 
Casting procedure
Casting procedure Casting procedure
Casting procedure
 
casting notes mpya.pptx
casting notes mpya.pptxcasting notes mpya.pptx
casting notes mpya.pptx
 
Casting Procedures and Defects
Casting Procedures and DefectsCasting Procedures and Defects
Casting Procedures and Defects
 
Casting procedure and casting defects
Casting procedure and casting defectsCasting procedure and casting defects
Casting procedure and casting defects
 

More from Jehan Dordi

More from Jehan Dordi (13)

Immediate Implants
Immediate ImplantsImmediate Implants
Immediate Implants
 
PROSTHODONTIC EVALUATION FOR IMPLANT TREATMENT PLANNING
PROSTHODONTIC EVALUATION FOR IMPLANT TREATMENT PLANNINGPROSTHODONTIC EVALUATION FOR IMPLANT TREATMENT PLANNING
PROSTHODONTIC EVALUATION FOR IMPLANT TREATMENT PLANNING
 
Smile Design
Smile DesignSmile Design
Smile Design
 
Geriatric Dentistry
Geriatric DentistryGeriatric Dentistry
Geriatric Dentistry
 
LASERS IN PROSTHODONTICS
LASERS IN PROSTHODONTICSLASERS IN PROSTHODONTICS
LASERS IN PROSTHODONTICS
 
Management of Kennedys Class III Classification
Management of Kennedys Class III ClassificationManagement of Kennedys Class III Classification
Management of Kennedys Class III Classification
 
Failures in Fixed Partial Denture
Failures in Fixed Partial DentureFailures in Fixed Partial Denture
Failures in Fixed Partial Denture
 
Occlusion in Complete Denture
Occlusion in Complete Denture Occlusion in Complete Denture
Occlusion in Complete Denture
 
RPI & RPA system
RPI & RPA systemRPI & RPA system
RPI & RPA system
 
Resisual Ridge Resorption
Resisual Ridge ResorptionResisual Ridge Resorption
Resisual Ridge Resorption
 
Examination &amp; diagnosis of edentulous patients
Examination &amp; diagnosis of edentulous patients Examination &amp; diagnosis of edentulous patients
Examination &amp; diagnosis of edentulous patients
 
Sterilization and Disinfection in Prosthodontics
Sterilization and Disinfection in ProsthodonticsSterilization and Disinfection in Prosthodontics
Sterilization and Disinfection in Prosthodontics
 
Blood and Blood related disorders
Blood and Blood related disordersBlood and Blood related disorders
Blood and Blood related disorders
 

Recently uploaded

Dehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service Dehradun
Dehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service DehradunDehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service Dehradun
Dehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service Dehradun
Sheetaleventcompany
 
Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...
Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...
Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...
Cara Menggugurkan Kandungan 087776558899
 
💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...
💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...
💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...
Sheetaleventcompany
 
Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...
Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...
Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...
dishamehta3332
 
Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...
Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...
Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...
Sheetaleventcompany
 
Control of Local Blood Flow: acute and chronic
Control of Local Blood Flow: acute and chronicControl of Local Blood Flow: acute and chronic
Control of Local Blood Flow: acute and chronic
MedicoseAcademics
 
Jual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan Cytotec
Jual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan CytotecJual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan Cytotec
Jual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan Cytotec
jualobat34
 
Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...
Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...
Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...
Sheetaleventcompany
 
Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...
Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...
Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...
Sheetaleventcompany
 
👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...
👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...
👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...
Sheetaleventcompany
 

Recently uploaded (20)

ANATOMY AND PHYSIOLOGY OF REPRODUCTIVE SYSTEM.pptx
ANATOMY AND PHYSIOLOGY OF REPRODUCTIVE SYSTEM.pptxANATOMY AND PHYSIOLOGY OF REPRODUCTIVE SYSTEM.pptx
ANATOMY AND PHYSIOLOGY OF REPRODUCTIVE SYSTEM.pptx
 
Dehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service Dehradun
Dehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service DehradunDehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service Dehradun
Dehradun Call Girl Service ❤️🍑 8854095900 👄🫦Independent Escort Service Dehradun
 
Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...
Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...
Cara Menggugurkan Kandungan Dengan Cepat Selesai Dalam 24 Jam Secara Alami Bu...
 
💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...
💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...
💚Chandigarh Call Girls 💯Riya 📲🔝8868886958🔝Call Girls In Chandigarh No💰Advance...
 
Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...
Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...
Whitefield { Call Girl in Bangalore ₹7.5k Pick Up & Drop With Cash Payment 63...
 
tongue disease lecture Dr Assadawy legacy
tongue disease lecture Dr Assadawy legacytongue disease lecture Dr Assadawy legacy
tongue disease lecture Dr Assadawy legacy
 
VIP Hyderabad Call Girls KPHB 7877925207 ₹5000 To 25K With AC Room 💚😋
VIP Hyderabad Call Girls KPHB 7877925207 ₹5000 To 25K With AC Room 💚😋VIP Hyderabad Call Girls KPHB 7877925207 ₹5000 To 25K With AC Room 💚😋
VIP Hyderabad Call Girls KPHB 7877925207 ₹5000 To 25K With AC Room 💚😋
 
Kolkata Call Girls Naktala 💯Call Us 🔝 8005736733 🔝 💃 Top Class Call Girl Se...
Kolkata Call Girls Naktala  💯Call Us 🔝 8005736733 🔝 💃  Top Class Call Girl Se...Kolkata Call Girls Naktala  💯Call Us 🔝 8005736733 🔝 💃  Top Class Call Girl Se...
Kolkata Call Girls Naktala 💯Call Us 🔝 8005736733 🔝 💃 Top Class Call Girl Se...
 
Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...
Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...
Dehradun Call Girls Service {8854095900} ❤️VVIP ROCKY Call Girl in Dehradun U...
 
Control of Local Blood Flow: acute and chronic
Control of Local Blood Flow: acute and chronicControl of Local Blood Flow: acute and chronic
Control of Local Blood Flow: acute and chronic
 
Genuine Call Girls Hyderabad 9630942363 Book High Profile Call Girl in Hydera...
Genuine Call Girls Hyderabad 9630942363 Book High Profile Call Girl in Hydera...Genuine Call Girls Hyderabad 9630942363 Book High Profile Call Girl in Hydera...
Genuine Call Girls Hyderabad 9630942363 Book High Profile Call Girl in Hydera...
 
Jual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan Cytotec
Jual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan CytotecJual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan Cytotec
Jual Obat Aborsi Di Dubai UAE Wa 0838-4800-7379 Obat Penggugur Kandungan Cytotec
 
Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...
Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...
Premium Call Girls Dehradun {8854095900} ❤️VVIP ANJU Call Girls in Dehradun U...
 
Ahmedabad Call Girls Book Now 9630942363 Top Class Ahmedabad Escort Service A...
Ahmedabad Call Girls Book Now 9630942363 Top Class Ahmedabad Escort Service A...Ahmedabad Call Girls Book Now 9630942363 Top Class Ahmedabad Escort Service A...
Ahmedabad Call Girls Book Now 9630942363 Top Class Ahmedabad Escort Service A...
 
Cardiac Output, Venous Return, and Their Regulation
Cardiac Output, Venous Return, and Their RegulationCardiac Output, Venous Return, and Their Regulation
Cardiac Output, Venous Return, and Their Regulation
 
🚺LEELA JOSHI WhatsApp Number +91-9930245274 ✔ Unsatisfied Bhabhi Call Girls T...
🚺LEELA JOSHI WhatsApp Number +91-9930245274 ✔ Unsatisfied Bhabhi Call Girls T...🚺LEELA JOSHI WhatsApp Number +91-9930245274 ✔ Unsatisfied Bhabhi Call Girls T...
🚺LEELA JOSHI WhatsApp Number +91-9930245274 ✔ Unsatisfied Bhabhi Call Girls T...
 
Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...
Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...
Call Girl In Indore 📞9235973566📞 Just📲 Call Inaaya Indore Call Girls Service ...
 
👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...
👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...
👉Chandigarh Call Girl Service📲Niamh 8868886958 📲Book 24hours Now📲👉Sexy Call G...
 
💰Call Girl In Bangalore☎️63788-78445💰 Call Girl service in Bangalore☎️Bangalo...
💰Call Girl In Bangalore☎️63788-78445💰 Call Girl service in Bangalore☎️Bangalo...💰Call Girl In Bangalore☎️63788-78445💰 Call Girl service in Bangalore☎️Bangalo...
💰Call Girl In Bangalore☎️63788-78445💰 Call Girl service in Bangalore☎️Bangalo...
 
Call 8250092165 Patna Call Girls ₹4.5k Cash Payment With Room Delivery
Call 8250092165 Patna Call Girls ₹4.5k Cash Payment With Room DeliveryCall 8250092165 Patna Call Girls ₹4.5k Cash Payment With Room Delivery
Call 8250092165 Patna Call Girls ₹4.5k Cash Payment With Room Delivery
 

Casting Procedures & Casting Defects in Dentistry

  • 1. CASTING PROCEDURES Presented by: Dr. Jehan Dordi I year MDS 1
  • 2. CONTENTS • Introduction • Sprue and Spruing • Crucible Former • Casting Ring • Casting Ring Liner • Investing • Shrinkage Compensation • Burnout Procedure • Casting machines • Casting Crucibles • Flux in Casting • Heat treatment 2
  • 3. • Casting Procedures • Divesting & Cleaning the casting • Finishing and polishing • Degassing Ceramo-metal casting • Casting defects • Review of Literature • References 3
  • 5. Terminology • Casting: It is defined as something that has been cast in a mold; an object formed by the solidification of a fluid that has been cast into a refractory mould (GPT-9). 5
  • 6. 3000 B.C- Copper was cast by Mesopotamian's 2500 B.C- Dental prosthesis fabricated from gold wire was found in Egypt 500 B.C.- Etruscans made bridges of soldered gold bands 1571- Benevento had done casting of both gold and bronze 1897- Phil brook described a method of casting metal in mould formed from a wax pattern for posterior tooth 1907- Taggart devised a practically useful casting machine 1928- The low heat casting technique was published by Coleman 1930- Carl Scheu, discovered the phenomena known as Hygroscopic Setting Expansion 1945- George D. Estes introduced the vacuum investing technique to prevent formation of air bubbles on surface of wax 1959- Strickland et al stated importance of type, shape & direction other than size of sprue 1959- Peyton stated tar flaring should occur at the sprue/ wax pattern junction 6
  • 7. The Lost Wax Process • The casting procedure by lost wax technique was introduced by Dr. William H. Taggart. • He introduced this technique and the casting machine in 1907 before the New York Odontological Group . • It soon led to the casting of inlays, onlays, clowns, fixed partial dentures (TPDs), and frameworks for removable partial dentures. Blowpipe Mould Compressed air cylinder 7
  • 8. Steps In Casting Procedure • Tooth/ teeth preparation • Impression • Die Preparation • Wax pattern fabrication • Spruing • Investing procedure • Burn out procedure • Casting • Divesting & Cleaning of the casting • Finishing of the casting 8
  • 10. Sprue • It is the channel or hole through which plastic or metal is poured or cast into a gate or reservoir and then into a mould. (GPT-9) Wax pattern attached to the crucible former with a sprue ready for investing. A ring liner is in place. 10
  • 11. Types of Sprue • According to material used: • Wax sprue former (for large restorations E.g.. RPD frameworks) • Plastic/Resin sprue former (smaller restorations) • Metal sprue ( smaller restorations E.g.. Crown) • According to process: • Prefabricated • Custom made • According to shape: • Solid • Hollow (Round) • According to the diameter of teeth: • For molars: 2.5mm (10-gauge) • For anteriors and pre-molars: 2.0mm (12-gauge) 11
  • 12. Materials Used In Sprue • Special wax supplied as rope form (rolls) of different diameters (gauges) for selection. • Hollow stainless steel wires of different diameters and lengths. • These are to be coated with thin layer of inlay wax by dipping in molten wax. • This is done for easy removal of sprue former after setting of investment. 12
  • 13. Length & Diameter of The Sprue • The length of the sprue former should be adjusted so that the pattern is approximately 6 mm from the open end of the ring. • The sprue former should be atleast 1.7mm in diameter unless the pattern is extremely small. • Sprue formers upto 2.5mm in diameter is used for very large patterns and bulky full crowns. 13
  • 14. Sprue Former Direction • It is attached at 45 degrees to the walls of the mould, which decreases the turbulence of molten alloy. 14
  • 15. Spruing Principles And Technique • The first step in the production of refractory mould is termed as spruing the pattern, whereby the wax pattern is attached to conical base by extension of wax, plastic, or metal. • This connector is known as sprue former, which should be properly selected in respect to size and configuration. 15
  • 16. Location Of Sprue • Sprue is attached to the bulkiest, non-critical part of the pattern. • Away from the margins and occlusal contacts. • Normally it is attached to largest non-functional cusp used. Wrong Correct 16
  • 17. Types of Spruing • Direct spruing: Sprue former provides direct connection between pattern area and the crucible former. • A basic weakness of direct spruing is the potential for suck back porosity at the junction of restoration and the sprue. • Indirect spruing: It uses the same basic principal of spruing. But the only difference lies in attachment of 3 running horizontal bars. The whole indirect sprue complex consists of 3 parts: 1. Feeder sprue 2. Horizontal running bar 3. 6 or 8 gauge sprue former 17
  • 18. Spruing The Pattern • Selection of sprue former depends on 1. type and size of the pattern and 2. the size of the ring used. • Long and thin sprue formers cause internal porosity. • This maybe overcome by using a reservoir or larger sprue. • Reservoir must have greater bulk than the adjacent portion of the pattern into which the sprue former is inserted. Reservoir 18
  • 19. Wax sprue-former length is checked before attachment to ensure that pattern is at least 3 to 6 mm from end of ring. 19
  • 20. • Any overheating of the wax could distort the pattern and hence hollow metal/plastic sprue formers are preferred, since they hold less heat than a solid sprue former. • The sprue former should be smooth and produce no sharp angles at the juncture of the wax pattern or the crucible former. Sprue former placement should provide smooth-flowing entry of gold into mold (arrows), with no sharp angles. Sprue former 20
  • 21. • Prefabricated sprue formers are available in a variety of sizes and configurations. • These plastic sprue formers are more rigid and decreases the chances of distorting the pattern. • A three-unit bridge and sprues with the “gate” technique, using prefabricated plastic formers is particularly useful for long-span multiple castings. Prefabricated plastic sprue formers Three-unit bridge and sprues with "gate" technique, using prefabricated plastic sprue former 21
  • 22. • Poor sprue designs can result in poor castings. • The sprue former must provide a proper in gate, allowing for smooth unobstructed flow of the molten gold into the mould. Poor sprue designs such as these can lead to casting failure. 22
  • 23. Spruing Metal-Ceramic Units • For small crowns a short, 8-gauge wax sprue former should be placed on the incisal edge so that the alloy may flow directly into the thinnest section of the casting. • The investment mold is generally about 1000° F (540°C) cooler than the molten alloy, and solidification occurs very quickly. Small units are easily cast by attaching short 6- or 8- gauge wax sprue former at incisal tip of wax pattern. 23
  • 24. • Movement of the liquid metal to the most distal margins of the casting must not be obstructed. • There should always be sufficient bulk of the sprue to allow for contraction of the metal during solidification without introduction of shrinkage porosity. • For larger castings (e.g., posterior crowns or small bridge units) an additional auxiliary sprue may be placed to facilitate filling the mould. Incomplete casting caused by excessively thin wax patterns and obstruction of gold flow in facial area of coping. 24
  • 25. • Small-diameter primary or auxiliary sprue formers attached to thicker sections of the casting will often cause shrinkage porosity. (A) Small primary sprue formers can create shrinkage porosity in casting. (B) Very thin auxiliary sprues can create regions of porosity in thicker sections of larger castings. 25
  • 26. • Large units are best sprued by the “gate” method, whereby a series of short 8-gauge wax sprue formers are attached to a continuous 6- or 8-gauge “ runner bar’ of wax or (preferably) plastic. 1. "Gate” spruing. A. Six- or eight-gauge sprue formers B. runner bar, 6-gauge or larger C. feeder sprues D. crucible former. 2 and 3, Four-unit bridge to be cast using prefabricated plastic "gate” sprue former. These rigid patterns help minimize wax distortion during investing procedures. 26
  • 27. • This runner bar in turn is attached to the crucible former by two or more large sprue formers, providing: 1. A minimum of distortion of the wax pattern, 2. A fairly uniform reservoir of metal near the entire casting, and 3. Even distribution of the alloy to all parts of the casting to minimize porosity. • For large castings, it is critical that the spruing arrangement provide a reservoir of metal that is external to the dental unit but positioned at the heat center of the investment mould. • Generally the alloy immediately adjacent to the walls of the mould will solidify first, the exposed surface of the button will solidify second, and the alloy internal to the mold will cool last. 27
  • 28. • If bulky pontics are placed at the heat center of the mould without a reservoir, porosity is very likely to occur in the pontic itself, resulting in a weak bridge. • Where a dental casting contains both thick and thin elements, porosity can be minimized by the addition of chill vents. • Chill vents accelerate the cooling of the pontic relative to the parts of the casting external to the dental unit itself. Addition of chill vents to bulky dental units may speed solidification and minimize porosity in the thick pontic or connector areas. Venting 28
  • 29. Spruing Of Cast Partial Framework Pattern • Spruing for casting of removable partial dentures involves a large quantity of metal, so special attention must be given to points of attachment, directions of the sprues, and the direction of flow of the molten metal. • A heavy sprue is an additional aid for offsetting the shrinkage. • It acts as a reservoir for the casting because its bulk remains molten longer than the rest of the casting and supplies molten metal to those areas that solidify and shrink first. 29
  • 30. • Mandibular casts are usually sprued through a hole in the center of the cast because it is easier to attach the sprue leads. • Maxillary casts are sprued the same way if the shape of the casting permits; otherwise, they are sprued from above. • Main and auxiliary sprues are attached to the central sprue approximately 7 mm below the tip of the central sprue. Wax pattern, not cast, is at least 7 mm from casting ring. A, Maxillary wax-up showing clearance. B, Mandibular wax-up centered in ring. 30
  • 31. Procedure: • Check the size of the investment cast in the investment flask. • When the wax pattern, is centered in the ring there should be at least 7-mm clearance between the wax pattern and the side of the ring. • Cut a 7-mm hole through the base of the cast in the center of the wax-up. • The hole can be started with a bur and completed with a knife blade. 31
  • 32. • Soften half a sheet of baseplate wax. Lay a straight hand-piece fissure bur on the edge of the wax, and roll the wax in a rod large enough to just pass through the hole in the base of the cast. A, Straight hand-piece fissure bur is laid on edge of half sheet of softened baseplate wax B, Wax is rolled around it to form rod large enough to just pass through hole in cast C, Wax sprue cone completed. 32
  • 33. • Push the wax rod through the base of the refractory cast until it protrudes from the other side about 10 mm. • Seal the rod to the cast with wax on both sides of the cast. • The rod protruding through the bottom of the cast will act as a handle during the investment procedure. 33
  • 34. • Use 8 or 10 gauge round wax for sprue leads on mandibular casts, and lay them directly on the surface of the cast. • Attach one end to the central sprue and the other to the bottom edge of the major connector. • An auxiliary lead is usually made of 14-gauge round sprue wax and is attached to the central sprue on the same level as the main sprues. • It should run as straight as possible and attach to the minor connector on the molar just below the occlusal rest or to the distal portion of the denture base. 34
  • 35. • Six-gauge half-round wax is most often used for sprue leads when spruing maxillary cast wax-ups. • Reinforce and smooth all junctions between the sprues and the framework patterns, and they are ready for investing 35
  • 37. Crucible Former • The base to which a sprue former is attached while the wax pattern is being invested in refractory investment; a convex rubber, plastic, or metal base that forms a concave depression or crucible in the refractory investment. (GPT-9) • The sprue is attached to a crucible former, usually made of rubber, which serves as a base for the casting ring during investing. • The exact shape of the crucible former depends on the type of ring and casting machine used. • With most modern machines, the crucible former is tall, to allow use of a short sprue and also to enable the pattern to be positioned near the end of the casting ring. Rubber crucible formers and corresponding casting rings. 37
  • 39. Casting Ring • Casting ring is a metal or silicone tube in which a refractory mold is made for casting dental restorations (GPT-9). • Investment material is poured in the casting ring and allowed to set around wax pattern. • Types of the casting ring: 1. Rubber ring 2. Metal ring 39
  • 40. TYPES OF RING ACCORDING TO SHAPE Round Oval COMPLETE RING Rigid Flexible SPLIT RING Metal Plastic 40
  • 42. Casting Ring Liner • Casting ring liners are the materials used to line casting ring so that during heating and expansion of the investment the compression of the liner should free the investment from the restraint of the ring. It is placed on inner side of the casting ring. • Types of Casting ring liner: 1. Asbestos 2. Non asbestos i. Fibrous ceramic aluminosilicate ii. Cellulose iii. Ceramic- Cellulose 42
  • 43. • The functions of liners are as follows: • To allow enough lateral expansion of mould (investment), during setting or heating. • Longer longitudinal expansion is reduced by adhesion of investment at the ends (3mm space). This minimizes the distortion. • When the ring is transferred from furnace to the casting machine it reduces the heat loss as it a thermal insulator. • Permits easy separation of the investment from the ring after casting process is over. 43
  • 44. • Formerly asbestos sheet liners were laid inside the casting ring leaving about 3mm at the ends. • Due to health hazards of inhaling asbestos dust or vapours which is carcinogenic, now cellulose or alumina silicate ceramic liners are used. Casting Ring Liner 44
  • 45. • If wetted these liners provide some extra water for the Hygroscopic Setting Expansion (HSE) of mould. Two or three layers give higher HSE of the mould laterally. • Split casting rings or plastic casting rings are used to get adequate lateral expansions specially for high fusing alloy. • In base metal alloy casting procedures ring-less casting investment is done. 45
  • 46. Ring-Less Casting System • A ring-less casting system provides maximum expansion of the investment. • This system, is called the Power Cast ring-less system (Whip-Mix Corporation, Louisville, USA), consists of three sizes of rings and formers, preformed wax sprues and shapes, investments powder and a special investment liquid. • The tapered plastic rings allow for removal of the investment mould after the material has set. • This system is suited for casting of alloys that require greater mould expansion than traditional gold based alloys. Crucible formers and cone-shaped plastic rings for a ringless investment technique in casting. The crucible former and plastic ring are removed before wax elimination, which leaves the invested wax pattern. The systems are designed to achieve expansion that is unrestricted by a metal ring. 46
  • 48. Investing • Investing: the process of covering or enveloping, wholly or in part, an object such as a denture, tooth, wax form, crown, etc., with a suitable investment material before processing, soldering, or casting. (GPT-9) 48
  • 49. 3 types of investments materials available: • Gypsum bonded investments: • For conventional casting of gold alloy inlays, • Onlays, • Crowns & FPD’s. • Phosphate bonded investments: • For metal ceramic restorations • Pressable ceramics & for base metal alloys. • Ethyl- silicate bonded investments: • For casting of removable partial dentures with base metal alloy. 49
  • 50. Preparatory Steps For Investing • First of all secure the wax pattern that is made. • A thin layer of special surfactant or wetting agents is applied, thin layer should be maintained which otherwise collect air bubble from the mix and cause nodule of casting. • Cleaning the wax pattern of debris or oil is done by surfactants which are available as: i. Pattern Cleanser ii. Diluted synthetic detergent solution iii. Debbublizer • The detergent material left behind reduces surface tension and causes better wetting. 50
  • 51. Investing Technique • There are two methods of investing 1. Hand mixing investing method 2. Vacuum mixing and investing 51
  • 52. Hand Mixing Investing Method • Required amount of distilled water (mixture of water + colloidal silica gel for phosphate bonded investment) is taken in a clean flexible bowl. • Weighed amount of powder is added and mixed thoroughly. • When a brush or small instrument is used to apply the investment material to the pattern, the wet material should be gently applied, pushed ahead of the applicator. (A)Paintbrush or small instrument is used to apply initial layer of investment over pattern; this procedure decreases chances of bubble entrapment inside pattern. (B), Remaining investment is then poured into ring, carefully, so as not to create voids in ring. 52
  • 53. • When the pattern is completely covered in this manner, the remaining investment is poured into the ring carefully to avoid entrapping air, and the investing procedure is completed. • A small amount of mix is painted on the surface of wax pattern for better wetting and then the remaining mix is vibrated into casting ring to fill completely. • Too much vibration causes sedimentation of larger investment particles, leaving thin mix close to the pattern, which may cause rough surface. 53
  • 54. Vacuum Mixing And Investing • Parts of machine: 1. Special investment mixing closed bowl, 2. Connection to evacuating pump, 3. A mixing pad connected to rotating shaft of an electric motor and 4. A side platform for resting the casting ring is used. • The proportioned material is taken in it, the speed and time of spatulations are adjusted to get mix of reproducible consistency. 54
  • 55. • After the casting ring has been filled with the investment material, any excess should be removed before the material sets. • The ring is now set aside to allow the investment material to complete its setting reaction and the accompanying setting expansion. 55
  • 56. Grinding the Investment • Carefully grind (on a model trimmer) or scrap the shiny skin off the end of the investment just prior to burn out. • Removes the impervious layer, opening the pores of the investment and facilitating gas release as the alloy is cast into the mold. • 3mm on each end is left as it serves to lock the investment within the ring & equalize radial & axial expansion. 56
  • 57. • The setting is completed in 30 to 40 minutes, at which time it may be placed in a burnout oven to eliminate the wax and obtain the remaining required thermal expansion. (According to “Philips Science of Dental Materials” the setting time is approximately one hour.) Before it starts to set, investment is wiped flush with top of ring. Any scraping attempted after set may fill in pores and inhibit gas escape from mold during casting. 57
  • 58. • When a hygroscopic technique is used, the freshly filled investment ring is immediately placed into a water bath for 30 minutes and kept at 100° F (38° C). • If metal sprue is used, it is pulled out easily, as exothermic reaction softens the wax coating. • The crucible formed is carefully cleaned by removing the loosely adhering investment particles which otherwise may fall into sprue and block it. Hygroscopic technique relies mainly on setting expansion to gain proper expansion of mold. After being filled, ring is immediately placed in constant temperature water bath at 100° F (38° C) for at least 30 minutes. 58
  • 60. Shrinkage compensation • The molten alloys used for dental restorations shrink upon solidification: gold alloys by approximately 1.5% and nickel-chromium alloys by as much as 2.4%. • If the mold is not made correspondingly larger than the original wax pattern, the resultant casting will be that much smaller. • For crowns, therefore, it is necessary to compensate for the solidification shrinkage of the specific alloy used by expanding the mold enough to at least equal the shrinkage. Four mechanisms to produce mold expansion: 1. Setting Expansion of Investment 2. Hygroscopic Expansion 3. Wax Pattern Expansion 4. Thermal Expansion 60
  • 61. • Setting Expansion: It is result of normal gypsum crystal growth. The expansion probably is enhanced by silica particles in the investment interfering with the forming crystalline structure of the gypsum, causing it to expand outward It occurs in small amount i.e. about 0.4% but is partly restricted by metal investment ring. • Hygroscopic Expansion: Maximum amount of expansion is by hygroscopic expansion. Water bath at 38°C is used, water in bath replaces water used by hydration process. Space between growing crystals is thus maintained. Crystals grow longer in outward direction causing expansion of mould. About 1.2 to 2.2% hygroscopic expansion takes place. More controlled amounts of hygroscopic expansion may be achieved by adding a measured amount of water to the setting investment 61
  • 62. • Wax pattern expansion: Expansion of the wax pattern while the investment is still fluid occurs when the wax is warmed above the temperature at which it was formed. The low-temperature burnout technique employs a combination of wax pattern expansion and thermal expansion of the mold. After the investment filled ring is removed from a 100°F (38°C) water bath, the ring is heated to only 900°F (482°C) before casting to produce the additional expansion needed. • Thermal expansion: Thermal expansion of the investment occurs when the investment is heated in the burnout oven. The investment around the wax pattern is allowed to harden in air at room temperature, and then it is heated to approximately 1200° F (650°C). At this temperature, the investment and metal ring expand enough to compensate for the shrinkage of the gold alloy. • When the investment has set, the layer at the top of the ring is trimmed off. • The rubber crucible former is removed, and any loose particles of investment are blown off. • The ring is then placed in the furnace for the recommended burnout schedule. 62
  • 64. Burnout procedure • Elimination of the wax pattern from the mould of set investment material is referred to as the burnout. • Ideally the casting ring containing the investment should be placed into the oven approximately 1 hour after investing the wax pattern. • If the burnout procedure must be delayed for several hours or overnight, it is advisable to place the invested pattern into a humidor to prevent excessive drying. Investment rings should be placed in humidor to prevent drying if it is anticipated that pattern will not be burned out for several hours or overnight. 64
  • 65. • To facilitate a rapid and clean burnout, the ring may be placed on a raised object within the oven. • A burnout started prematurely may cause fine cracks in the gypsum-bonded investment. • Once the heating is initiated, the casting should be completed without permitting the mold to cool. Porcelain tooth placed in bottom of oven provides good support for one edge of ring, allowing molten wax and gases to escape freely. Cracks, caused by expanding steam, occur when damp investment is heated too rapidly. This is major cause of fins on castings 65
  • 66. • The mold should be placed in an oven preheated to approximately 900° F (480° C), held at that temperature for 20 minutes, and the temperature then raised slowly to 1290° F (700° C) and held for 30 minutes. • Prolonged heating above 1290° F should be avoided. • Gypsum-bonded investments will break down at this temperature, and the Sulphur and chlorine will contaminate the gold alloy as it enters the mould. • With a quartz investment, the rate of heating should be carefully controlled, since rapid heating will produce a larger casting than will slow heating. 66
  • 68. Classification Of Casting Machines • Based on methods of casting the machines are: 1. Centrifugal force type 2. Air pressure type 3. Vacuum type • Based on heating system employed: 1. Torch melted 2. Induction melted 3. Arc melted 68
  • 69. Casting Machines • Alloys are melted in one of the four following ways, depending on the available types of casting machines: 1. The alloy is melted in a separate crucible by a torch flame and cast into the mold by centrifugal force. 2. The alloy is melted electrically by a resistance heating or induction furnace and then cast into the mold centrifugally by motor or spring action. Centrifugal casting machine, spring wound. Spring-wound casting machine with electrical resistance melting furnace. 69
  • 70. 3. The alloy is melted by induction heating and then cast into the mold centrifugally by motor or spring action. 4. The alloy is vacuum-arc melted and cast by pressure in an argon atmosphere. Induction melting casting machine with induction coil Vacuum-arc Melting Machine 70
  • 71. Torch Melting/Centrifugal Casting Machine • The casting machine spring is first wound from two to five turns. • The alloy is melted by a torch flame in a glazed ceramic crucible attached to the “broken arm” of the casting machine. • The broken arm feature accelerates the initial rotational speed of the crucible and casting ring, thus increasing the linear speed of the liquid casting alloy as it moves into and through the mold. • Once the metal has reached the casting temperature and the heated casting ring is in position, the machine is released and the spring triggers the rotational motion 71
  • 72. Counter Weight Tongs Broken arm Crucible former Platform for casting ring Hinge for rotation 72
  • 73. Zones of Flame • Mixtures of natural gas and air, or oxyacetylene gases are used. • Zone 1 - Non combustion zone/ Mixing Zone • Zone 2 - Combustion zone • Zone 3 - Reducing zone • Zone 4 - oxidizing zone 73
  • 74. Electrical Resistance–Heated Casting Machine • In this device, current is passed through a resistance heating conductor, and automatic melting of the alloy occurs in a graphite or ceramic crucible. • This is an advantage, especially for alloys such as those used for metal-ceramic prosthesis, which are alloyed with base metals in trace amounts that tend to oxidize on overheating. 74
  • 75. Induction Melting Machine • With this unit, the alloy is melted by an induction field that develops within a crucible surrounded by water-cooled metal tubing. • The electric induction furnace is a transformer in which an alternating current flows through the primary winding coil and generates a variable magnetic field in the location of the alloy to be melted in a crucible. • Once the alloy reaches the casting temperature in air or in vacuum, it is forced into the mold by centrifugal force, air pressure, or vacuum. 75
  • 76. Direct-Current Arc Melting Machine • The direct-current arc is produced between two electrodes: the alloy and the water-cooled tungsten electrode. • The temperature within the arc exceeds 4000 °C and the alloy melts very quickly. • This method poses a high risk of overheating the alloy, and damage may result after only a few seconds of prolonged heating. 76
  • 77. Vacuum or Pressure-Assisted Casting Machine • For this machine, the molten alloy is heated to the casting temperature, drawn into the evacuated mold by gravity or vacuum, and subjected to additional pressure to force the alloy into the mould. • For titanium and titanium alloys, vacuum arc heated- argon pressure casting machines are required. 77
  • 79. Casting Crucible • It is a vessel or container made of any refractory material (frequently ceramics) used for melting or calcining any substance that requires a high degree of heat. (GPT- 9) 79
  • 80. • Following are the types of crucible used for casting: 1. Clay crucible (for many of the crown and bridge alloys, such as the high noble and noble types) 2. Carbon crucible (For high noble crown and bridge alloys but also for the higher-fusing gold-based metal-ceramic alloys) 3. Quartz crucible (for high-fusing alloys of any type) 4. Ceramic crucible (For palladium-silver and nickel or cobalt based alloys) 80
  • 82. Flux in casting • A reducing flux should be used in melting the alloy. • The flux (50% boric acid powder and 50% fused borax) increases the fluidity and reduces the potential for oxidation. • Flux maybe added to: 1. To minimizing porosity. 2. To increase fusing of metal. 3. Prevent oxidation. 82
  • 84. Heat Treatment • To adequately resist excessive wear, restoration must be returned to a hardened state prior to its clinical use. • The physical properties, specifically the mechanical properties of some gold alloys, may be modified by heat treatment. • Gold alloys containing 7% or more copper will respond to heat treatment by changes in microstructure, and consequently in their handling properties. 84
  • 85. • Softening heat treatment consists of heating the alloy to 1290° F (700° C) and maintaining that temperature for approximately 15 minutes, followed by quenching in room-temperature water. • Hardening heat treatment may be conducted in either of two ways: 1. Heat soaking at a constant temperature of approximately 840° F (450° C) for 15 minutes 2. Low cooling from 840° to 480° F (450° to 250° C) over a period of 15 minutes, followed by quenching in water. 85
  • 87. Casting Procedures: Low-fusing Gold Alloys • To melt low-fusing gold alloy for the casting procedure, three methods are available: 1. Compressed air and gas, 2. Oxygen and gas, or 3. An electric casting machine. 87
  • 88. • When a torch is used flame cone should be approximately 40 mm. • The tip of the reducing cone is used to make a rapid and clean melt. • Electric furnace casting machine eliminates the need for a torch and the judgment required in heating the gold alloy. It is well controlled, accurate, and precise. Properly adjusted torch. (A) Reducing zone is used to melt gold. (B)Oxidizing zone is cooler than reducing zone and will not heat gold to proper casting temperature. Electric casting machine 88
  • 89. • If the investment cools prior to the casting, the mold will become smaller through cooling contraction of the investment. • Castings produced with large amounts of alloy will usually produce better detail and definition than minimum amounts of metal used. • If melted in a reducing flame, molten gold alloy that has reached the proper temperature for casting will appear shiny with a mirror like surface. When gold has reached proper temperature for casting, it will be elliptic with well-rounded edges, yellow-orange in color, and will appear to be “spinning.” 89
  • 90. • When the alloy has solidified and cooled for approximately 1 minute, the investment may be placed into room-temperature water, and the alloy quenched. • This will aid in removing the adhering investment, which can be cleaned from the casting with a laboratory brush, toothbrush, or an air abrasive. Pencil-type abrasive blasters can be used to remove investment and oxides from casting without appreciable danger of damaging margins. 90
  • 91. Casting High-Fusing Metal-Ceramic Alloys • Casting of porcelain-bonding alloys requires that the metal be heated approximately 212° F (100° C) higher than its upper melting point. • This is generally in the range of 2200° to 2500° F (1200° to 1370° C). • These temperatures can be achieved with 1. A gas-oxygen torch or 2. By induction heating. 91
  • 92. Induction Casting • Induction casting can be used for alloys of any composition and provides for excellent control of the casting temperature. • The alloy is rapidly melted in a carbon crucible, heated by electrical induction. • The atmosphere is reducing, and at casting the molten alloy temperature is centrifugally cast into the mold. • The apparatus for induction casting is expensive. 92
  • 93. Torch Casting • All alloys can be cast with a gas-oxygen or oxy-acetylene torch. • The casting of porcelain-bonding alloys differs from casting low-fusing gold alloys in the following respects: 1. No asbestos is used in the high-heat crucibles, since it may react with the alloy constituents at high temperatures. 2. The technician should have one high-heat crucible for each brand of alloy being cast in order to avoid cross-contamination. 3. No casting flux is used on porcelain-bonding alloys, since flux may alter its composition and diminish the bond strength. This is particularly true of gold alloys. 4. The visual clues for assessing casting temperatures are different from low-fusing gold alloys, since high-fusing alloys are heated white-hot before they are released into the mold. 93
  • 94. 5. Greater casting pressures (i.e., the number of turns of a centrifugal machine) are generally required to force the porcelain-bonding alloy into the mold. • When a multiple-sprue technique is used, the inlets should be aligned for the fastest and most uniform distribution of alloy within the mold. • The sprue and button should be sufficient to provide for cooling dynamics that do not lead to shrinkage porosity. 94
  • 95. • High-fusing gold alloys will melt into a pool that is cast when it has reached a white-hot, almost vaporous state. • Nonprecious nickel-chromium alloys are generally supplied as sharp cornered ingots of various shapes and are heated until the corners round over. When gold alloy is ready to cast it will be white hot, forming smooth oxide-free elliptical pool. A, Base metal ingot— beginning of melt with gas-oxygen flame. B, Ingot continues to melt. C, Base metal ingot ready to cast. Corners and sharp edges have rounded. D, Base metal ingot overheated, produces changes in composition and excessive oxidation. 95
  • 96. • All alloys should be melted as quickly as possible to avoid excessive oxidation. • High-fusing gold alloys are least sensitive to overheating or prolonged heating. • After casting, the machine should be allowed to spin freely until it has nearly stopped . • It may then be braked still, and the ring removed and promptly quenched in water. • The investment is initially removed by carving and breaking it off the casting, taking care not to damage the casting. Investments must be carefully broken away from casting. Attention to proper investing and casting procedures will allow for clean separation of casting from investment 96
  • 97. Casting of Titanium alloys • Advantages of titanium and titanium alloys include excellent biocompatibility and corrosion resistance, which results from the presence of a thin, adherent, passivating surface layer of titanium dioxide. • The dental casting of titanium and titanium alloys poses special problems because of the high melting point of titanium (1668°C) and its strong tendency to oxidize and react with other materials. • Titanium dental casting machines that represent a substantial expense must provide either a vacuum environment or an argon atmosphere. • Both vacuum/argon pressure and centrifugal casting machines have been developed, and both argon-arc melting and induction melting have been used to fuse titanium and titanium alloys. 97
  • 98. • Patterns for casting are coated, and investments must be used to provide the appropriate expansion. • Reaction of titanium or titanium alloy with the investment (and perhaps with the residual atmosphere in the casting machine) results in a very hard near-surface region (termed α case) that can exceed 50 μm in thickness. • Currently, titanium castings of clinically acceptable accuracy can be produced, whereby the marginal fit of cast complete crowns is superior to that for titanium crowns milled by the computer-aided design/computer assisted manufacturing (CAD/CAM) technique. 98
  • 100. Quenching • After the casting has solidified, the ring is removed and quenched in water as soon as the button exhibits a dull-red glow. • Two advantages are gained in quenching: 1. The noble metal alloy is left in an annealed condition for burnishing, polishing, and similar procedures, and 2. When the water contacts the hot investment, a violent reaction ensues, resulting in a soft, granular investment that is easily removed. 100
  • 101. Pickling • Often the surface of the casting appears dark with oxides and tarnish, such surface can be removed by a process known as pickling. • Pickling consists of heating the discolored casting in an acid. • One of the best pickling solutions for gypsum-bonded investments is a 50% hydrochloric acid solution. • Nonprecious nickel-chromium alloys must never be placed in acid because of their high reactivity. • The hydrochloric acid aids in the removal of any residual investment, as well as of the oxide coating. 101
  • 102. • 'The best method for pickling is to place the casting in a test tube or dish and to pour the acid over. • The pickling solution should be renewed frequently, because it is likely to become contaminated after reusing the solution several times. • In no case should the casting be held with steel tongs so that both the casting and the tongs come into contact with the pickling solution, because this may contaminate the casting. • When the steel tongs contact electrolyte, a small galvanic cell is created and copper is deposited on the casting at the point where the tongs grip it which becomes future source for discoloration in the area. 102
  • 103. Sandblasting • The process of altering the surface of a material through the use of abrasive particles propelled by compressed air or other gases. (GPT-9). • It can be done using a high speed sandblaster. • Most common medium for sandblasting in dentistry is aluminum oxide. • The fine aluminum oxides are recycled within the sandblasting machine and replaced after 30- 40 minutes of total accumulated operation time. • 60-80 psi of force is exerted by the machine. 103
  • 104. • Provides mechanical retention between porcelain-metal by removing the casting oxides as well as proper sandblasting of the alloy with 100-150 microns aluminum oxide results to mechanical bonding. • Also provides micromechanical retention of denture base to framework. • Two types of sandblasting 1. Automatic sandblaster 2. Blast cabinets 104
  • 105. Cleaning The Casting • The first step is to thoroughly clean the surfaces of all residual investment. • Abrasive blasting is effective for this. • The blasting medium can become embedded in the surface and be a source of contamination if not thoroughly removed. • Traces of investment can easily be ground into the metal surface and act as sources of gas at the porcelain -metal interface when porcelain is added. Residual investment (I) is easily removed from casting (C) by use of Al203 or glass bead powders in pencil- tip air-abrasive units. Margins are easily protected by using this type apparatus . 105
  • 106. • Resin-bound abrasives (e.g., some carborundum or paper disks) can contaminate the metal surface with resin, leading to severe bubbling when porcelain is added. • Once the porcelain-bearing surface is clean, it may optionally be sandblasted with a clean 25 to 50 µm aluminum oxide abrasive to texturize it. Contamination of metal surface by finishing with resin bound abrasives can lead to severe bubbling in porcelain. This layer must be removed with hydrofluoric acid and metal refinished with no contaminating, ceramic-bound abrasives. 106
  • 107. • This will increase the area of bonding and improve the wettability of the metal. • Surface roughness is not necessary to achieve a satisfactory porcelain-to-metal bond, since the main mode of attachment is chemical, not mechanical • The casting can now be cleaned in distilled water in an ultrasonic cleaner. • When the metal surface is absolutely clean — free of oxides, investment and organic films — it is ready for the next stage of metal conditioning (finishing). Aluminum oxide air- abrasion of metal surface after finishing with ceramic -bound stones will produce uniform texture and improve wettability by opaque porcelain. 107
  • 109. Objectives And Procedures • The objectives and procedures for finishing are different for each part of the cast restoration. • Zone 1 is the internal margin • Zone 2 the internal surface • Zone 3 the sprue • Zone 4 the proximal contacts • Zone 5 the occlusal surface • Zone 6 the axial walls and • Zone 7 the external margins. 109
  • 110. Zone 1: Internal Margin Objective: • To minimize any dissolution of the luting agent, a 1- mm wide band of metal must be closely adapted to the tooth surface. • A discrepancy within this zone can significantly reduce a restoration’s longevity. • Good adaptation is obtained by careful reflowing of the wax pattern. Reflowing of the wax pattern. The objective is to create a well-adapted 1-mm zone to prevent cement dissolution. Proper reflowing before investing is essential. 110
  • 111. Procedure for Zone-1 • If a defect occurs in the marginal area, the restoration must be remade. • Even small nodules can prevent a casting from seating completely. • Small nodules, if far enough away from the margin itself, can be removed under a binocular microscope with exceptionally cautious use of small rotary instruments (e.g., a No. 1/2 round bur). 111
  • 112. Zone 2: Internal Surface (Intaglio) Objective: • No contact should exist between the die and the internal surface (intaglio) of the casting. • A uniform space of 25 to 35 μm is necessary for the luting agent to spread evenly. • Any contacts must be identified and relieved by careful selective grinding of the internal surface. 112
  • 113. Procedure for Zone-2 • Casting’s internal surface should, be examined for nodules before the restoration is seated on the die. • Even a very small nodule can result in significant increase of the marginal gap width. • Any significant force will abrade or chip the die, so that the casting will seat on the die but will not seat fully on the prepared tooth. 113
  • 114. • Once the casting has been adjusted, determining the exact location of the nodule is no longer possible. • Therefore, the nodule should be removed entirely in one step, rather than through sequential relief of the internal surface. • Several agents are commercially available to facilitate identification of the seating interference between the casting and the die. When a nodule is removed, removal of slightly more than the defect ensures complete seating of the restoration. 114
  • 115. A, Incomplete seating. B, Liquid marking agent. C, A thin coat is applied to the internal surface and air dried. D, The casting is gently returned to the die. E, The area of interference is identified. F, Nodules are best removed with a small round bur. G, Seated casting. A B C D EFG 115
  • 116. Zone 3: The Sprue Objective • To re-establish proper coronal structure and function, the sprue must be sectioned, and the casting must be recontoured in the area of its attachment. Procedure for Zone- 3: • Once the fit of the casting has been verified on the die and it has been found to be acceptable, the sprue is sectioned, and the area of its attachment to the casting is reshaped. 116
  • 117. (A)Attached sprue to casting (B)cut around the sprue and then twist it off. (C)With multiple castings made simultaneously, care must be taken not to damage the margin inadvertently. (D)Disks and stones are used for gross recontouring. B C A D 117
  • 118. Zone 4: Proximal Contacts Objective • The proximal contact areas are adjusted in the laboratory so that they will be correct (or slightly too tight) when the casting is evaluated in the patient’s mouth. 118
  • 119. Procedure for Zone-4 • The proximal contacts on the stone cast can be minimally relieved by careful scraping with a scalpel. • When proximal contacts are adjusted, placing a thin articulating film between adjacent castings or between the casting and the adjacent tooth is helpful. • Doing this allows the areas where binding contact occurs to be adjusted through selective adjustment where markings result. 119
  • 120. A, Thin articulating film interposed between a metal-ceramic restoration and the adjacent tooth. B, The area of contact that prevents complete seating is readily apparent. C, Articulating film is used to detect the location of an excessive proximal contact on cast metal. A B C 120
  • 121. Zone 5: Occlusal Surface Objective • Occlusal contacts are re-established in static and dynamic relationships to the opposing arch. • Obtaining accurate and stable contacts does not require highly polished metal occlusal surfaces; a satin finish is acceptable. • Occlusal form must ensure positional stability and satisfy all functional requirements. 121
  • 122. Procedure for Zone-5 • The occlusal contacts are checked with thin articulating film to ensure that they match the design in the waxing stage. • If an occlusal contact is heavy in wax, it springs back slightly when the articulator is opened and produces an occlusal prematurity in the casting. A and B, Occlusal prematurity's are generally the result of excessively heavy contact on the wax pattern. B A 122
  • 123. • Occlusal adjustments can be performed with flame shaped finishing burs or diamond bur. • The correct technique for occlusal adjustment is to re-develop the anatomy of the entire ridge or cusp rather than grinding only the point of interference. • Simultaneously, any nodules can be removed, and grooves can be defined with a finishing bur or a small round bur. A, Occlusal adjustment is readily accomplished with a pointed diamond or carbide bur. B, The grooves and fissures are concurrently refined. B A 123
  • 124. • Before starting any adjustment, the practitioner should use a thickness gauge on the metal. • If only minimum clearance was established at the tooth preparation stage, indiscriminate adjustment leads to inadequate thickness of the casting. As occlusal adjustments are made (A), the residual thickness is continually monitored with an appropriately designed thickness gauge (B). For structural durability, metal thickness of less than 1.0 mm is inadequate and is the result of insufficient occlusal reduction. 124
  • 125. • If the wax pattern has been carefully finished, a smooth casting results, and removing surface oxides with a soft wire brush wheel is sufficient. • The surface can then be polished with rouge on a soft brush wheel (which removes only 5 μm from the surface of the casting. A, Initially a wire brush is used on the occlusal surfaces. B, A fine-grit sandpaper disk is applied for removing pits and irregularities from the axial walls C A rubber wheel is then used on the axial walls. D, Castings, after polishing with buffing compound, immediately before clinical evaluation. E The completed castings immediately before cementationE DC BA 125
  • 126. Zone 6: Axial Walls Objective • When axial wall finishing is completed, the walls should be smoothly contoured and highly polished, enabling the patient to perform optimum plaque control. 126
  • 127. Procedure for Zone-6 • Surface defects are removed by grinding with abrasive particles bound into a grinding stone or rubber wheel, on a paper disk, or applied as an abrasive paste. • A sequence of progressively finer grades is used to attain the desired surface. (A)Carborundum disks and stones of varying degrees of coarseness are typically used first; (B)these are followed by garnet paper and sandpaper disks, (C)rubber points and white Arkansas stones, (D)and rubber wheels and points, along with small carbide burs for removing nodules. C B D A 127
  • 128. • The most efficient method of polishing is to use a sequence of progressively finer abrasives each removing the scratches made by the previous grade. • Time is wasted if the progression to a finer grade abrasive is too rapid because the coarser grits remove material much more efficiently. A, Assorted abrasives, sandpaper disks, rubber points, and polishing wheels. B, Instruments used range from small carbides (for removing nodules) and a steel wire brush (for occlusal surface smoothing) to buffing wheels and compounds. C, A coarse wheel is used to true and thin the edge of a rubber wheel. D, Buffing compounds applied on a wheel or bristle brush. A D B C 128
  • 129. Zone 7: External Margins Objective • Margin finishing is crucial for a restoration’s longevity and therefore merits special attention. • The objective of all cast restoration finishing is a highly polished metal surface without ledges or steps as the transition is made from restoration to unprepared tooth. • Failure to accomplish this leads to compromised plaque control. 129
  • 130. Procedure for Zone-7 • Where access allows, cavo-surface margins should be finished directly on the tooth. A Supragingival margins allow access for finishing the restoration directly on the tooth. B, Fine-grit white stone lubricated with petroleum jelly. C, Rubber point. D, Completed restoration. A C D B 130
  • 131. A. When subgingival margins do not allow access, final finishing is performed on the die. During final polishing, the margin is carefully supported with a finger. B. Carefully rubbing a smooth instrument along the length of the margin (burnishing). C. Gently brushing a fine-grit stone over the surface to remove casting roughness Using a soft rubber wheel or point. CBA 131
  • 133. Degassing Ceramometal Castings • After the coping or framework is cleaned, it should be subjected to a degassing or surface – conditioning treatment. • During degassing the unit is heat treated to remove contaminants from the surface or possibly to remove entrapped gas from the alloy . • In addition, a thin oxide film is formed on the surface. This film is essential to porcelain bonding. • Precious gold alloys should be rapidly heated in air to 1950° F (1065° C ), held there 5 to 10 minutes , and rapidly cooled to room temperature. 133
  • 134. • The unit will have darkened due to surface oxidation . • Semiprecious and base metal alloys are generally heated to 1950° F , and held at this temperature in a 25- to 28- inch (64- to 70- cm) mercury vacuum for 5 to 10 minutes. • At this temperature the vacuum can be broken and the unit then cooled quickly. This procedure will produce a thin but sufficient oxide coating on the metal surface. • A second aluminium oxide (Al2O3) abrasive blasting of the surface is recommended for base metal alloys to remove excessive oxidation. 134
  • 136. Casting Defects • Defects in castings can be classified under four headings: 1. Distortion; 2. Surface roughness and irregularities; 3. Porosity and 4. Incomplete or missing detail 136
  • 137. Distortion • Distortion of the casting is probably related to a distortion of the wax pattern, it can be minimized by proper manipulation of the wax and handling of the pattern. • The setting and hygroscopic expansions of the investment may produce a non-uniform expansion of the walls of the pattern. • Factors that affect distortion are: 1. The configuration of the pattern, 2. The type of wax, and 3. The thickness influence the distortion that occurs • Distortion increases as the thickness of the pattern decreases, the lower is the setting expansion of the investment, the less lower is distortion. 137
  • 138. Surface Roughness, Irregularities, And Discoloration • Surface roughness is defined as relatively finely spaced surface imperfections whose height, width, and direction establish the predominant surface pattern. • Surface irregularities are isolated imperfections, such as nodules, that are not characteristic of the entire surface area. • Improper technique can lead to a marked increase in surface roughness as well as to the formation of surface irregularities. 138
  • 139. • Surface discoloration and roughness can result from sulfur contamination. • The interaction of the molten alloy with sulfur produces a black or gray layer on the surface of gold alloys that is brittle and does not clean readily during pickling. A black-coated noble metal alloy casting resulting from sulfur contamination or oxidation during melting of the alloy. 139
  • 140. Air Voids • Small nodules on a casting are caused by air bubbles that become attached to the pattern during or subsequent to the investing procedure. • The best method to avoid air bubbles is to use the vacuum investing technique. • A wetting agent may be helpful in preventing the collection of air bubbles on the surface of the pattern. • It is best to air-dry the wetting agent, because any excess liquid dilutes the investment, possibly producing surface irregularities on the casting. 140
  • 141. Water Films • Wax is repellent to water; if the investment becomes separated from the wax pattern in some manner, a water film may form irregularly over the surface. • If the pattern is slightly moved, jarred, or vibrated after investing or if the painting procedure does not result in intimate contact of the investment with the pattern, such a condition may result. • If too little water is used, the investment may be un- manageably thick, so that it cannot be properly applied to the pattern. • A wetting agent is useful for the prevention of such irregularities. 141
  • 142. Foreign Bodies • When foreign substances get into the mold a surface roughness may be produced • A rough crucible former with investment clinging to it may roughen the investment on its removal so that bits of investment are carried into the mold with the molten alloy. • Usually contamination results not only in surface roughness but also in incomplete areas or surface voids. • Any casting that shows sharp, well-defined deficiencies indicates the presence of some foreign particles in the mold, such as pieces of investment and bits of carbon from a flux. • Bright-appearing concavities may be the result of flux being carried into the mould with the metal. 142
  • 143. Impact Of Molten Alloy On The Mold Wall • The direction of the sprue former should be such that the molten gold alloy does not impact a weak portion of the mould surface. • Sometimes the abraded area is smooth, so that it cannot be detected on the surface of the casting. • Such a depression in the mould is reflected as a raised area on the casting, which prevents complete seating of the casting. • It can be avoided by proper spruing so as to prevent the direct impact of the molten metal at an angle of 90° to the investment surface. 143
  • 144. Pattern Position • If several patterns are invested in the same ring, they should not be placed too close together. • Likewise, positioning too many patterns in the same plane in the mould should be avoided. • The expansion of wax is much greater than that of the investment, and this may cause breakdown or cracking of the investment if the spacing between patterns is less than 3 mm. 144
  • 145. Carbon Inclusions • Carbon from a crucible, an improperly adjusted torch, or a carbon-containing investment, can be absorbed by the alloy during casting. • These particles may lead to the formation of carbides or even create visible carbon inclusions. 145
  • 146. Porosity • Porosity may occur both within the interior region of a casting and in the external surface which results in surface roughness. • Internal porosity weakens the casting and also cause discoloration. • If severe, it can cause plaque accumulation at the tooth-restoration interface, and secondary caries or periodontal disease may result within the adjacent tooth structure. • Although porosity in a casting cannot be prevented entirely, it can be minimized by the use of proper techniques. 146
  • 147. Porosities in noble metal alloy castings are classified below. • Solidification defects A. Localized shrinkage porosity B. Microporosity C. Suck-back porosity • Trapped gases A. Pinhole porosity B. Gas inclusions C. Subsurface porosity D. Back pressure porosity 147
  • 148. Localized Shrinkage • Generally caused by premature termination of the flow of molten metal during solidification. • Continual feeding of molten metal through the sprue must occur to make up for the shrinkage of metal volume during solidification. • Localized shrinkage generally occurs near the sprue-casting junction. • If the sprue freezes in its cross section before this flow is completed, a localized shrinkage void will occur in the last portion of the casting that solidifies. Localized shrinkage porosity in pontic of three-unit bridge caused by delayed solidification and lack of a chill-set sprue. 148
  • 149. Microporosity • Microporosity occurs from solidification shrinkage. • It occurs when the solidification is too rapid for the micro-voids to segregate to the liquid pool. • This premature solidification causes the formation of small, irregular voids. • Such phenomena can occur from rapid solidification if the mold or casting temperature is too low. 149
  • 150. Pinhole- Porosity • Oxygen is dissolved by some of the metals, while they are in the molten state. • During solidification, the gas is expelled to form blebs and pores in the metal. • The porosity that extends to the surface is usually in the form of small pinpoint holes. • When the surface is polished, other pinholes appear. 150
  • 151. Gas Inclusion Porosity • The gas inclusion porosities are usually much larger than pinhole porosity. • Larger spherical porosities can be caused by gas occluded from a poorly adjusted torch flame or by use of the mixing or oxidizing zones of the flame rather than the reducing zone. • If the alloy has been used before, these types of porosities can be minimized by pre-melting and correctly adjusting and positioning the torch flame during melting. 151
  • 152. Subsurface Porosity • They may be caused by the simultaneous nucleation of solid grains and gas bubbles at the first moment that the alloy freezes at the mould walls. • This type of porosity can be diminished by controlling the rate at which the molten metal enters the mould. 152
  • 153. Suck-Back Porosity • It occurs externally, usually in the interior of a crown near the area of the sprue, if a hot spot has been created by the hot metal impinging from the sprue channel on a point of the mould wall. • The entering metal impinges onto the mold surface at this point and creates a higher localized mold temperature in this region, known as a hot spot. • This hot spot causes the local region to freeze last and results in what is called suck-back porosity. • Suck-back porosity often occurs at an occluso-axial line angle or inciso-axial line angle that is not well rounded. 153
  • 154. • A hot spot may retain a localized pool of molten metal after other areas of the casting have solidified. • This, in turn, creates a shrinkage void or suck back porosity. • This type of porosity defect can be eliminated by flaring the point of sprue attachment and reducing the mold-melt temperature differential—that is, lowering the casting temperature by about 30 °C. 154
  • 155. Back-Pressure Porosity • Entrapped air bubbles on the inner surface of the casting, are sometimes referred to as back-pressure porosity. • This is caused by the inability of the air in the mold to escape through the pores in the investment or by the pressure gradient that displaces the air pocket toward the end of the investment via the molten sprue and button. • Frequently found at the cavity surface of a crown or mesio- occlusal-distal casting. • It can be prevented by use of the dense modern investments, by an increase in mold density produced by vacuum investing, and by the tendency for the mold to clog with residual carbon when the low-heat technique is used. 155
  • 156. Incomplete Casting • The obvious cause is that the molten alloy has been prevented in some manner from completely filling the mould. • At least two factors that may inhibit the ingress of the liquefied alloy are insufficient venting of the mold and high viscosity of the fused metal. • The first consideration, insufficient venting, is directly related to the back pressure exerted by the air in the mould. • If the air cannot be vented quickly, the molten alloy does not fill the mold before it solidifies. • These failures are usually exemplified by rounded, incomplete margins. 156
  • 157. • A second common cause of an incomplete casting is incomplete elimination of wax residues from the mold. • If too many products of combustion remain in the mold, the pores in the investment may become filled, so that the air cannot be vented completely. Incomplete casting resulting from incomplete wax elimination is characterized by rounded margins and shiny appearance. 157
  • 159. Type of Failure Procedural Errors Solution Suck-back porosity Sprue attached at a right angle to the wax pattern, creating a “hot spot” Sprue should always be attached at the bulkiest portion of the wax pattern directed at 45° to the surface Improper margin fit Improper handling of wax pattern during removal from the oral cavity Hard wax can be used for wax pattern fabrication. Careful handling of the pattern during removal along the path of insertion, taking care not to disturb the margins Air bubble in the Casting Air bubble entrapment during investing procedure Prevented by carrying out the mixing and investing procedure under vacuum 159
  • 160. Type of Failure Procedural Errors Solution Water film Pattern is slightly moved, jarred, or vibrated after investing Prevented by proper use of a wetting agent and proper care of the invested casting ring Contamination of the alloy Reaction of the alloy with crucible used Crucible unable to withstand the temperature Choose appropriate crucible for each alloy Microporosities Solidification occurs too rapidly (when the mold or casting temperature is too low) Proper temperature to be maintained 160
  • 161. Type of Failure Procedural Errors Solution Pits in casting • Debris in mould • Dirty wax • Loose debris in crucible • Mould temperature too hot • Join ingate, sprue former, and pattern with continuous smooth surface with no jagged areas of investment to be broken off and pushed into mold ahead of alloy • Use only clean, new wax for patterns and sprue formers • Use clean crucible for each casting • Lower burnout temperature since too high temperature causes investment breakdown, producing weak surface easily abraded by alloy Fins on castings • Over vibration during investment or disturbing ring during set • Heating ring too rapidly causes moisture in mold to form steam and rupture out mold • Avoid over vibration and place investment ring in area free from disturbances until investment is completely set • Heat mold slowly. 161
  • 162. Type of Failure Procedural Errors Solution Localized shrinkage porosity & Incomplete casting • Using a sprue with a very small diameter • Discrepancy in temperatures between the casting ring/ mold and the molten alloy • Insufficient casting pressure during the casting process • Incomplete elimination of wax and incomplete venting • Higher viscosity of the molten alloy Larger sprue diameter to allow proper flow of molten metal into the mold • Sprue to be attached at the bulkiest portion of the wax pattern directed at 45° to the surface • Proper balance between mold and molten alloy temperatures • Pressure on the arm of the casting machine should be maintained for at least 4 sec to allow the alloy to fill the mould • A vent of 0.5 mm in diameter should be provided to allow escape of gases • Proper casting temperature of the molten metal to be maintained during casting Contamination of the casting The casting held with steel tongs during pickling Use of steel tongs should be avoided 162
  • 163. Type of Failure Procedural Errors Solution Rounded margins • Incomplete burnout of wax pattern • Insufficient heating of alloy before casting • Margins melted while attaching pattern to sprue or former • Improper diameter/length of sprue restricts flow of alloy into mold; metal freezes before margins are complete • Heat soak mould for 1 hour at minimum of 950° F (510° C) to ensure elimination of carbon residue • Heat alloy to 150° F (57° C) above fusion temperature at moment of casting alloy • Keep pattern and sprue former in horizontal position when attaching, so that heat rising from instrument does not soften pattern • Average casting should have 10-gauge sprue approximately 6 mm long 163
  • 164. Type of Failure Procedural Errors Solution Rough surface on casting • Excess moisture on pattern • Water-powder ratio too high in mixing investment • Too much casting pressure, causing investment breakdown from force of alloy • Prolonged overheating of gypsum- bound investment • Remove all moisture from pattern, sprue former, and ring • Use correct water-powder ratio • Do not wind machine too tightly • Use correct heating cycle for burnout procedure; do not heat above 1290° F (700° C) 164
  • 166. Lombardas P, Carbunaru A, McAlarney ME, Toothaker RW, of Dental S, Oral Surgery NY. Dimensional accuracy of castings produced with ringless and metal ring investment systems. The Journal of prosthetic dentistry. 2010 Jul 1;84(1):27 31. • Lombardas et al did a study to determine “Dimensional accuracy of castings produced with ringless and metal ring investment systems” • This study compared the vertical margin accuracy of lost wax castings produced with the conventional casting technique using a metal ring and a technique that uses a ringless system. • From copings fabricated on a metal die, 1. 30 castings were produced from a high palladium alloy for metal ceramic restorations 2. 10 castings were cast with phosphate-bonded investment with the ringless technique 3. 10 were cast with the phosphate-bonded investment with a metal ring, and 4. The final 10 were cast using Hi-temp (Whip Mix) phosphate-bonded investment with a metal ring. 166
  • 167. • The internal surface of the castings were not modified before seating with finger pressure. For vertical margin discrepancy measurements, an optical microscope at a magnification of 100× was used. Data were analyzed with 1-way ANOVA (repeated measures) and the Student test. • When following the manufacturers’ recommendations, the castings of the ringless technique provided less vertical margin discrepancy (mean value 181 ± 71 μm) than the castings produced with the conventional metal ring technique (290 ± 87 μm and 291 ± 88 μm). The difference was significant (P<.001) 167
  • 168. • Within the conditions of this study, the following conclusions were drawn: 1. The vertical margin discrepancy of the ringless group for the buccal, the lingual, and the distal sites were significantly less than that of the 2 ring groups (P<.001). 2. There was no significant difference of the vertical margin discrepancy between the 2 metal ring groups. 3. There was no significant difference in the vertical margin discrepancy at the buccal, lingual, mesial, and distal surfaces within the same group. 4. The ringless technique was clinically acceptable and can be used for the fabrication of fixed prosthodontic restorations. 168
  • 169. Prabhu KG, Eswaran MA, Phanikrishna G, Deepthi B. Sprue design alterations and its effect on the properties of base metal alloy castings: An in vitro study. Journal of pharmacy & bioallied sciences. 2015 Aug;7(Suppl 2):S524. • Prabhu et al did a study on to evaluate “Sprue design alterations and its effect on the properties of base metal alloy castings: An in vitro study.” • To study the effect of various sprue designs on the properties of base metal alloy castings. The base metal alloys are extensively used for their excellent properties such as an increase in hardness, high melting range, high elastic modulus, its compatibility with ceramic material and low cost. • However, to improve the properties of the base metal alloys is leading to various modifications in their fabrication procedure – which include sprue designs and their mode of attachment to the wax pattern. 169
  • 170. • Study compared the effect of three sprue designs on the properties of mass and micro-hardness of base metal alloy castings. viz. 1. Conical sprue, 2. Cylindrical sprue and 3. Bottleneck sprue • A prefabricated wax mesh pattern was selected for the fabrication of the alloy test samples in the study. • The cylindrical sprue design was connected to the mesh pattern with a straight attachment. • The bottleneck sprue design was connected to the mesh pattern with a constricted attachment. • The conical sprue design was connected to the mesh pattern with a flared attachment. • In this manner, ten samples for each of the three different sprue designs were prepared. 170
  • 171. • Results: The obtained value for mass and microhardness were subjected to statistical analysis. ANOVA test was performed to determine the difference between the sprue designs. • Conclusion: The bottleneck sprue, conical sprue, and cylindrical sprue designs did not exert any apparent influence on the mass and microhardness. 171
  • 172. Earnshaw R. The effect of casting ring liners on the potential expansion of a gypsum-bonded investment. Journal of dental research. 2010 Nov;67(11):1366- 70. • Earnshaw R. did a study to determine “The effect of casting ring liners on the potential expansion of a gypsum-bonded investment” • A study was conducted on cellulose paper, ceramic paper and asbestos paper of the effects on the setting and subsequent thermal expansion of a gypsum-bonded cristobalite casting investment. • Thermal expansion measurements were made on the same specimens that were produced during the setting expansion tests. • Control specimens setting against a smooth dry surface showed a total expansion of 1. 7%. Specimens setting against dry ceramic liners had similar total expansions, in the range 1. 6 to 1. 7%. • Specimens setting against either of the wet lining materials showed an increased total expansion (in the range 2.2 to 2.3%), by virtue mainly of a large increase in setting expansion. 172
  • 173. • Dry asbestos and dry cellulose liners gave higher expansions than pre-wetted ones, since they abstracted water from the mix, reducing its effective W/P ratio (giving a thicker mix), and then functioned as wet liners. • These results suggest that, at least as far as potential investment expansion is concerned, wet cellulose liners have an effect similar to that of the traditional wet asbestos liners. • Dry ceramic liners give a much lower investment expansion, and when these liners are used, an investment with an increased measured expansion could be an advantage. 173
  • 174. Baskaran BE, Prabhu KG, Prabhu R, Krishna GP, Eswaran MA, Gajapathi B. Casting made simple using modified sprue design: An in vitro study. Indian Journal of Dental Research. 2014 May 1;25(3):340. • Baskaran et al did a study on “Casting made simple using modified sprue design: An in vitro study”. • Regardless of the alloy used for casting, the casting technique should yield a casted alloy, which should possess sufficient mass, surface hardness and minimal porosity after casting. • Twenty patterns for casting were made from three-dimensional printed resin pattern simulating a 3 unit FPD and casted using modified sprue technique. • Later test samples were cemented sequentially on stainless steel model using pressure indicating paste and evaluated for vertical marginal gap in eight predetermined reference areas. 174
  • 175. • Marginal gap were measured in microns using Video Measuring System. A portion of the axial wall of the cast abutments depicting premolar and molar were sectioned and embedded in acrylic resin and tested for micro hardness and porosity. • The results obtained for marginal gap, micro hardness, and porosity of all test samples were tabulated, descriptive statistics were calculated and the values were found to be within the clinically acceptable range. • Thus new sprue technique can be an alternative and convenient method for casting which would minimize metal wasting and less time consuming. 175
  • 176. REFERENCES • Kenneth J. Anusavice. Philip’s Science of Dental Material. 11th Edition. St. Louis, Missouri: Saunders Elsevier; 2003. • Rosenstiel, Land, Fujimoto. Contemporary Fixed Prosthodontics. 5th Edition. St. Louis Missouri: Saunders Elsevier; 2016. • Herbert T Shillingburg, David Sather, Joseph Cain, Luis Blanco. Fundamentals of Fixed Prosthodontics. 4th Edition. Hanover Park, Illinois, USA: Quintessence Publishing Co, Inc; 2012. • Robert Marrow, Kenneth Rudd, John Rhoads. Dental Laboratory Procedures Volume II. 2nd Edition. St. Louis, Missouri: Mosby; 1986 • V Shama Bhat, Nandish BT. Science of Dental Materials. 2nd Edition. Delhi: CBS Publishers; 2013 • S Mahalaxmi. Materials used in dentistry. 1st Edition. Haryana: Wolters Kluwer Health; 2013 176
  • 177. • Robert Marrow, Kenneth Rudd, John Rhoads. Dental Laboratory Procedures Volume III. 2nd Edition. St. Louis, Missouri: Mosby; 1986 • Lombardas P, Carbunaru A, McAlarney ME, Toothaker RW, of Dental S, Oral Surgery NY. Dimensional accuracy of castings produced with ringless and metal ring investment systems. The Journal of prosthetic dentistry. 2010 Jul 1;84(1):27 31. • Earnshaw R. The effect of casting ring liners on the potential expansion of a gypsum-bonded investment. Journal of dental research. 2010 Nov;67(11):1366-70. • Prabhu KG, Eswaran MA, Phanikrishna G, Deepthi B. Sprue design alterations and its effect on the properties of base metal alloy castings: An in vitro study. Journal of pharmacy & bioallied sciences. 2015 Aug;7(Suppl 2):S524. • Baskaran BE, Prabhu KG, Prabhu R, Krishna GP, Eswaran MA, Gajapathi B. Casting made simple using modified sprue design: An in vitro study. Indian Journal of Dental Research. 2014 May 1;25(3):340. 177

Editor's Notes

  1. Distance between highest point on wax pattern and open end of ring is minimum 6mm
  2. Name of special wax
  3. Buccal cusp of upper posterior teeth Lingual cusp of lower posterior teeh
  4. Gate technique ????
  5. Debbublizer contains Citric acid Sodium 2 phenylpropane 2-sulfonate Propane 1-2 diol (propylene glycol)
  6. Air and gas are mixed here. No heat present. Dark in colour Green in colour….zone of partial combustion & has oxidizing nature Blue zone. Hottest part of flame. Used for fusion of casting alloy Final combustion between gas and surrounding air occurs. Not used for fusion
  7. Precious (gold - platinum-palladium ) gold alloys can be soaked in hydrofluoric acid or substitutes to help remove investment. Semiprecious alloys ( gold-silver palladium or silver - palladium ) should only be acid treated.