Al6061 Nanoindentation results

317 views

Published on

Al6061 Nanoindentation results

Published in: Engineering
  • Login to see the comments

  • Be the first to like this

Al6061 Nanoindentation results

  1. 1. Al6061 NI results NIST Project Ali Khosravani Jordan Weaver
  2. 2. 4 5 6 7 8 -3 x 10 50 55 60 65 0.6 0.5 0.4 0.3 0.2 0.1 0 -0.1 70 Fit4 Average Abs Residual E eff h-change Fit4 Max Abs Residual 0.023 0.022 0.021 0.02 0.019 0.018 0.017 0.016 0.015 0.014 Aged at 400F for 2hrs_ 100micron tip_001
  3. 3. AR_ 100micron tip_ test 001 40 20 0 65 70 75 80 Modulus [GPa] 40 20 0 0.96 0.98 1 1.02 R2 40 20 0 40 60 80 100 Modulus Length [#points] 40 20 0 -0.7 -0.6 -0.5 -0.4 -0.3 H r [nm] 50 0 0.009 0.01 0.011 0.012 0.013 Fit1 Avg.Abs.Res. 40 20 0 0.02 0.03 0.04 0.05 0.06 Fit1 Max.Abs.Res. 40 20 0 0.1 0.11 0.12 0.13 Fit2 Avg.Abs.Res. 40 20 0 0.25 0.3 0.35 0.4 0.45 Fit2 Max.Abs.Res. 50 0 0.5 0.6 0.7 0.8 0.9 h change [nm/nm] 0.4 0.5 0.6 0.7 40 20 0 P change [mN/mN] 6 6.5 7 7.5 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 40 20 0 0.018 0.02 0.022 0.024 Fit4 Max.Abs.Res. 40 20 0 0.2 0.21 0.22 0.23 P* [mN] 40 20 0 18.5 19 19.5 h* [nm] 0 1 2 3 -3 x 10 20 10 0 dP [mN] 40 20 0 -0.2 -0.1 0 0.1 0.2 dH [nm] effective sample Fit1 Fit2 Fit3
  4. 4. AR_ 100micron tip_ test 001 Estat = mean: 74.0953 median: 74.5196 stdev: 1.4504 min: 70.4381 max: 75.9712 Ystat = mean: 0.5090 median: 0.5134 stdev: 0.0169 min: 0.4678 max: 0.5321 Hstat = mean: 26.4590 median: 26.6196 stdev: 0.5423 min: 25.0907 max: 27.1902 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=70.4792; Bunge=0, 0, 0; Strength=0.50739; Hardening=26.4099 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 300 250 200 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 5 10 15 4 x 10 0 -0.5 -1 -1.5 -2 -2.5 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.2 0.4 0.6 0.8 8 6 4 2 0 -2 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  5. 5. AR_ 100micron tip_ test 003 40 20 0 66 68 70 72 74 76 Modulus [GPa] 200 100 0 0.95 0.96 0.97 0.98 0.99 1 R2 0 50 100 150 100 50 0 Modulus Length [#points] 100 50 0 -2 -1.5 -1 -0.5 0 H r [nm] 0 0.01 0.02 0.03 0.04 100 50 0 Fit1 Avg.Abs.Res. 0 0.05 0.1 0.15 0.2 200 100 0 Fit1 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 100 50 0 Fit2 Avg.Abs.Res. 0 0.5 1 1.5 100 50 0 Fit2 Max.Abs.Res. 0 0.2 0.4 0.6 0.8 100 50 0 h change [nm/nm] 100 50 0 0.1 0.2 0.3 0.4 0.5 0.6 P change [mN/mN] 4 5 6 7 8 -3 x 10 100 50 0 Fit4 Avg.Abs.Res. 100 50 0 0.012 0.014 0.016 0.018 0.02 0.022 Fit4 Max.Abs.Res. 100 50 0 0.2 0.4 0.6 0.8 1 P* [mN] 100 50 0 14 16 18 20 22 24 h* [nm] 0 1 2 3 4 -3 x 10 40 20 0 dP [mN] 100 50 0 -0.6 -0.4 -0.2 0 0.2 0.4 dH [nm] effective sample Fit1 Fit2 Fit3
  6. 6. AR_ 100micron tip_ test 003 Estat = mean: 72.8881 median: 72.7568 stdev: 1.7132 min: 70.0032 max: 75.9966 Ystat = mean: 0.5726 median: 0.5718 stdev: 0.0247 min: 0.4797 max: 0.6337 Hstat = mean: 25.9397 median: 25.8888 stdev: 0.6667 min: 24.6468 max: 27.2296 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.6 1.4 1.2 1 0.8 0.6 0.4 0.2 0 Ind. Strain Ind. Stress [GPa] Es=69.4139; Bunge=0, 0, 0; Strength=0.58068; Hardening=25.8184 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 2.5 5 x 10 1 0 -1 -2 -3 -4 -5 -6 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  7. 7. AR_ 100micron tip_ test 004 20 10 0 65 70 75 80 Modulus [GPa] 40 20 0 0.99 0.995 1 1.005 R2 40 20 0 110 120 130 140 150 Modulus Length [#points] 20 10 0 -1.4 -1.2 -1 -0.8 -0.6 H r [nm] 40 20 0 0.008 0.01 0.012 0.014 Fit1 Avg.Abs.Res. 40 20 0 0.02 0.04 0.06 0.08 Fit1 Max.Abs.Res. 0.2 0.25 0.3 0.35 40 20 0 Fit2 Avg.Abs.Res. 40 20 0 0.5 1 1.5 Fit2 Max.Abs.Res. 40 20 0 -0.1 0 0.1 0.2 0.3 h change [nm/nm] 0 0.05 0.1 0.15 0.2 20 10 0 P change [mN/mN] 20 10 3.8 4 4.2 4.4 4.6 -3 x 10 0 Fit4 Avg.Abs.Res. 50 0 0.011 0.012 0.013 0.014 0.015 Fit4 Max.Abs.Res. 40 20 0 0.35 0.4 0.45 0.5 P* [mN] 40 20 0 22 22.5 23 23.5 24 h* [nm] 0 1 2 3 4 -3 x 10 20 10 0 dP [mN] 40 20 0 -0.2 0 0.2 0.4 0.6 dH [nm] effective sample Fit1 Fit2 Fit3
  8. 8. AR_ 100micron tip_ test 004 Estat = mean: 72.9264 median: 72.7957 stdev: 1.7328 min: 70.0236 max: 75.9430 Ystat = mean: 0.5620 median: 0.5603 stdev: 0.0253 min: 0.5206 max: 0.6081 Hstat = mean: 25.3096 median: 25.2949 stdev: 0.6958 min: 24.1726 max: 26.5177 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=69.3459; Bunge=0, 0, 0; Strength=0.55924; Hardening=25.3294 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 5 x 10 1 0 -1 -2 -3 -4 -5 -6 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 20 15 10 5 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  9. 9. AR_ 100micron tip_ test 005 20 10 0 66 68 70 72 74 76 Modulus [GPa] 100 50 0 0.95 0.96 0.97 0.98 0.99 1 R2 40 20 0 20 40 60 80 100 120 Modulus Length [#points] 50 0 -0.7 -0.6 -0.5 -0.4 -0.3 H r [nm] 4 6 8 10 -3 x 10 50 0 Fit1 Avg.Abs.Res. 100 50 0 0.01 0.02 0.03 0.04 0.05 Fit1 Max.Abs.Res. 100 50 0 0.08 0.1 0.12 0.14 0.16 Fit2 Avg.Abs.Res. 200 100 0 0.25 0.3 0.35 0.4 0.45 Fit2 Max.Abs.Res. 0 0.2 0.4 0.6 0.8 40 20 0 h change [nm/nm] 0 0.1 0.2 0.3 0.4 0.5 40 20 0 P change [mN/mN] 4 5 6 7 8 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 40 20 0 0.016 0.018 0.02 0.022 Fit4 Max.Abs.Res. 50 0 0.25 0.3 0.35 0.4 0.45 P* [mN] 100 50 0 18.5 19 19.5 20 20.5 21 h* [nm] 0 1 2 3 4 -3 x 10 20 10 0 dP [mN] 40 20 0 -0.4 -0.2 0 0.2 0.4 dH [nm] effective sample Fit1 Fit2 Fit3
  10. 10. AR_ 100micron tip_ test 005 Estat = mean: 72.9738 median: 73.0464 stdev: 1.7727 min: 70.0284 max: 75.9751 Ystat = mean: 0.5677 median: 0.5668 stdev: 0.0264 min: 0.5105 max: 0.6133 Hstat = mean: 24.2864 median: 24.3030 stdev: 0.6177 min: 23.2218 max: 25.3615 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=69.4103; Bunge=0, 0, 0; Strength=0.56771; Hardening=24.2611 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 5 10 15 4 x 10 0.5 0 -0.5 -1 -1.5 -2 -2.5 -3 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 10 8 6 4 2 0 -2 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  11. 11. AR_ 100micron tip_ test 006 10 5 0 65 70 75 80 Modulus [GPa] 20 10 0 0.94 0.96 0.98 1 R2 10 5 0 20 30 40 50 60 Modulus Length [#points] 20 10 0 -0.6 -0.5 -0.4 -0.3 -0.2 H r [nm] 4 5 6 7 -3 x 10 20 10 0 Fit1 Avg.Abs.Res. 20 10 0 0.005 0.01 0.015 0.02 0.025 Fit1 Max.Abs.Res. 20 10 0 0.08 0.1 0.12 0.14 Fit2 Avg.Abs.Res. 10 5 0 0.2 0.3 0.4 0.5 Fit2 Max.Abs.Res. 20 10 0 -0.5 0 0.5 1 h change [nm/nm] 0 0.2 0.4 0.6 0.8 20 10 0 P change [mN/mN] 4 5 6 7 -3 x 10 20 10 0 Fit4 Avg.Abs.Res. 10 5 0 0.01 0.015 0.02 Fit4 Max.Abs.Res. 20 10 0 0.2 0.25 0.3 0.35 0.4 P* [mN] 20 10 0 10 11 12 13 14 h* [nm] 0 1 2 3 4 -3 x 10 10 5 0 dP [mN] 20 10 0 -0.2 0 0.2 0.4 0.6 dH [nm] effective sample Fit1 Fit2 Fit3
  12. 12. AR_ 100micron tip_ test 006 Estat = mean: 72.7770 median: 72.6317 stdev: 1.6269 min: 70.0297 max: 75.9841 Ystat = mean: 1.3887 median: 0.5726 stdev: 0.8684 min: 0.4794 max: 2.3706 Hstat = mean: -20.5747 median: 24.3717 stdev: 46.3225 min: -68.8533 max: 25.6614 1.6 1.4 1.2 1 0.8 0.6 0.4 0.2 0 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 Ind. Strain Ind. Stress [GPa] Es=69.1032; Bunge=0, 0, 0; Strength=0.55979; Hardening=25.303 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 300 250 200 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 5 10 15 4 x 10 0 -0.5 -1 -1.5 -2 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.2 0.4 0.6 0.8 10 8 6 4 2 0 -2 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  13. 13. AR_ 100micron tip_ test 007 20 10 0 65 70 75 80 Modulus [GPa] 40 20 0 0.985 0.99 0.995 1 1.005 R2 20 10 0 90 100 110 120 Modulus Length [#points] 20 10 0 -0.9 -0.8 -0.7 -0.6 -0.5 H r [nm] 20 10 0 0.01 0.015 0.02 Fit1 Avg.Abs.Res. 20 10 0 0.03 0.04 0.05 0.06 Fit1 Max.Abs.Res. 0.2 0.25 0.3 0.35 20 10 0 Fit2 Avg.Abs.Res. 0 0.5 1 1.5 20 10 0 Fit2 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 20 10 0 h change [nm/nm] 0 0.05 0.1 0.15 0.2 20 10 0 P change [mN/mN] 40 20 5.5 6 6.5 7 -3 x 10 0 Fit4 Avg.Abs.Res. 20 10 0 0.016 0.018 0.02 0.022 Fit4 Max.Abs.Res. 20 10 0 0.48 0.5 0.52 0.54 0.56 P* [mN] 20 10 0 18 18.5 19 19.5 h* [nm] 0 2 4 6 -3 x 10 20 10 0 dP [mN] 40 20 0 -0.5 0 0.5 dH [nm] effective sample Fit1 Fit2 Fit3
  14. 14. AR_ 100micron tip_ test 007 Estat = mean: 72.2464 median: 71.9764 stdev: 1.6662 min: 70.0129 max: 75.9662 Ystat = mean: 0.5074 median: 0.5047 stdev: 0.0193 min: 0.4798 max: 0.5531 Hstat = mean: 25.7443 median: 25.7191 stdev: 0.7086 min: 24.5450 max: 27.1741 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=68.7734; Bunge=0, 0, 0; Strength=0.50939; Hardening=25.8316 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 5 x 10 1 0 -1 -2 -3 -4 -5 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 20 15 10 5 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  15. 15. AR_ 100micron tip_ test 009 20 10 0 66 68 70 72 74 76 Modulus [GPa] 40 20 0 0.96 0.97 0.98 0.99 1 1.01 R2 20 10 0 40 60 80 100 120 Modulus Length [#points] 20 10 0 -0.8 -0.6 -0.4 -0.2 0 H r [nm] 5 6 7 8 9 10 -3 x 10 20 10 0 Fit1 Avg.Abs.Res. 50 0 0.01 0.02 0.03 0.04 0.05 Fit1 Max.Abs.Res. 20 10 0 0.11 0.12 0.13 0.14 0.15 0.16 Fit2 Avg.Abs.Res. 20 10 0 0.2 0.4 0.6 0.8 1 Fit2 Max.Abs.Res. 10 5 0 -0.05 0 0.05 0.1 0.15 0.2 h change [nm/nm] 0 0.05 0.1 0.15 0.2 10 5 0 P change [mN/mN] 4 5 6 7 -3 x 10 20 10 0 Fit4 Avg.Abs.Res. 10 5 0 0.014 0.016 0.018 0.02 0.022 0.024 Fit4 Max.Abs.Res. 40 20 0 0.25 0.3 0.35 0.4 0.45 P* [mN] 40 20 0 14 15 16 17 18 h* [nm] 0 1 2 3 4 -3 x 10 10 5 0 dP [mN] 40 20 0 -0.4 -0.2 0 0.2 0.4 dH [nm] effective sample Fit1 Fit2 Fit3
  16. 16. AR_ 100micron tip_ test 009 Estat = mean: 72.3650 median: 72.3985 stdev: 1.6707 min: 70.0855 max: 75.9545 Ystat = mean: 0.6027 median: 0.6021 stdev: 0.0314 min: 0.5364 max: 0.6666 Hstat = mean: 25.0466 median: 25.0440 stdev: 0.5939 min: 24.1868 max: 26.2760 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=68.8635; Bunge=0, 0, 0; Strength=0.60705; Hardening=25.0446 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 5 x 10 1 0 -1 -2 -3 -4 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 14 12 10 8 6 4 2 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  17. 17. AR_ 100micron tip_ test 010
  18. 18. AR_ 100micron tip_ test 010 Estat = mean: 72.5138 median: 72.2047 stdev: 1.5804 min: 70.0063 max: 75.9970 Ystat = mean: 1.1205 median: 1.1902 stdev: 0.2391 min: 0.3946 max: 1.3185 Hstat = mean: 10.6983 median: 8.5662 stdev: 5.5002 min: 8.2477 max: 27.3548
  19. 19. 400F_ 100micron tip_ test 001 40 20 0 66 68 70 72 74 76 Modulus [GPa] 400 200 0 0.95 0.96 0.97 0.98 0.99 1 R2 40 20 0 60 80 100 120 Modulus Length [#points] 40 20 0 -6 -4 -2 0 H r [nm] 0 0.05 0.1 0.15 0.2 0.25 100 50 0 Fit1 Avg.Abs.Res. 0 0.2 0.4 0.6 0.8 100 50 0 Fit1 Max.Abs.Res. 0 0.2 0.4 0.6 0.8 1 100 50 0 Fit2 Avg.Abs.Res. 0 1 2 3 4 50 0 Fit2 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 50 0 h change [nm/nm] 0 0.1 0.2 0.3 0.4 50 0 P change [mN/mN] 100 50 0 0.005 0.01 0.015 0.02 Fit4 Avg.Abs.Res. 40 20 0 0.01 0.02 0.03 0.04 0.05 Fit4 Max.Abs.Res. 0 2 4 6 8 50 0 P* [mN] 0 20 40 60 50 0 h* [nm] 0 0.01 0.02 0.03 0.04 0.05 40 20 0 dP [mN] 40 20 0 -1.5 -1 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  20. 20. 400F_ 100micron tip_ test 001 Estat = mean: 72.7560 median: 72.6725 stdev: 1.7194 min: 70.0141 max: 75.9311 Ystat = mean: 0.5800 median: 0.5799 stdev: 0.0273 min: 0.5142 max: 0.6424 Hstat = mean: 25.7733 median: 25.7376 stdev: 0.8190 min: 23.9460 max: 27.7413 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=69.1823; Bunge=0, 0, 0; Strength=0.60068; Hardening=25.4006 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 5 0 -5 -10 6 -1 0 1 2 3 5 x 10 -15 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 4 50 40 30 20 10 0 P 2/3 h Modulus Fit Data Elastic 0 0.02 0.04 0.06 0.08 0.1 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  21. 21. 400F_ 100micron tip_ test 002 40 20 0 66 68 70 72 74 76 Modulus [GPa] 200 100 0 0.95 0.96 0.97 0.98 0.99 1 R2 50 0 60 80 100 120 Modulus Length [#points] 50 0 -6 -4 -2 0 H r [nm] 0 0.05 0.1 0.15 0.2 100 50 0 Fit1 Avg.Abs.Res. 0 0.2 0.4 0.6 0.8 50 0 Fit1 Max.Abs.Res. 0 0.2 0.4 0.6 0.8 1 100 50 0 Fit2 Avg.Abs.Res. 0 1 2 3 4 50 0 Fit2 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 0.5 50 0 h change [nm/nm] 0 0.1 0.2 0.3 0.4 50 0 P change [mN/mN] 100 50 0 0.005 0.01 0.015 0.02 Fit4 Avg.Abs.Res. 40 20 0 0.015 0.02 0.025 0.03 0.035 0.04 Fit4 Max.Abs.Res. 0 2 4 6 40 20 0 P* [mN] 0 10 20 30 40 50 40 20 0 h* [nm] 0 0.01 0.02 0.03 0.04 0.05 40 20 0 dP [mN] 40 20 0 -2 -1 0 1 2 dH [nm] effective sample Fit1 Fit2 Fit3
  22. 22. 400F_ 100micron tip_ test 002 Estat = mean: 72.5480 median: 72.3265 stdev: 1.7056 min: 70.0063 max: 75.9879 Ystat = mean: 0.6048 median: 0.6052 stdev: 0.0245 min: 0.5445 max: 0.6608 Hstat = mean: 26.2425 median: 26.1201 stdev: 0.7859 min: 24.9040 max: 28.0767 1.5 1 0.5 0 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 Ind. Strain Ind. Stress [GPa] Es=68.8711; Bunge=0, 0, 0; Strength=0.61391; Hardening=25.8814 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 2 0 -2 -4 -6 -8 -10 6 -1 0 1 2 3 5 x 10 -12 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 4 40 30 20 10 0 P 2/3 h Modulus Fit Data Elastic 0 0.2 0.4 0.6 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  23. 23. 400F_ 100micron tip_ test 003 20 10 0 65 70 75 80 Modulus [GPa] 100 50 0 0.94 0.96 0.98 1 R2 40 20 0 80 90 100 110 120 Modulus Length [#points] 40 20 0 -4 -3 -2 -1 0 H r [nm] 0 0.02 0.04 0.06 0.08 40 20 0 Fit1 Avg.Abs.Res. 0 0.1 0.2 0.3 0.4 40 20 0 Fit1 Max.Abs.Res. 0 0.2 0.4 0.6 0.8 50 0 Fit2 Avg.Abs.Res. 0 1 2 3 40 20 0 Fit2 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 40 20 0 h change [nm/nm] 0 0.05 0.1 0.15 0.2 100 50 0 P change [mN/mN] 40 20 0 0.005 0.01 0.015 Fit4 Avg.Abs.Res. 40 20 0 0.01 0.02 0.03 0.04 Fit4 Max.Abs.Res. 0 1 2 3 4 20 10 0 P* [mN] 0 10 20 30 40 40 20 0 h* [nm] 0 0.02 0.04 0.06 40 20 0 dP [mN] 20 10 0 -0.5 0 0.5 1 1.5 dH [nm] effective sample Fit1 Fit2 Fit3
  24. 24. 400F_ 100micron tip_ test 003 Estat = mean: 73.0235 median: 73.0678 stdev: 1.7908 min: 70.0025 max: 75.9985 Ystat = mean: 0.5911 median: 0.5877 stdev: 0.0241 min: 0.5384 max: 0.6472 Hstat = mean: 26.7180 median: 26.7403 stdev: 0.7762 min: 25.1076 max: 28.2214 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.6 1.4 1.2 1 0.8 0.6 0.4 0.2 0 Ind. Strain Ind. Stress [GPa] Es=69.6973; Bunge=0, 0, 0; Strength=0.57997; Hardening=27.0297 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 5 0 -5 -10 -15 6 -2 0 2 4 5 x 10 -20 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 2 4 6 50 40 30 20 10 0 -10 P 2/3 h Modulus Fit Data Elastic 0 0.1 0.2 0.3 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  25. 25. 400F_ 100micron tip_ test 004 20 10 0 66 68 70 72 74 76 Modulus [GPa] 40 20 0 0.97 0.98 0.99 1 1.01 R2 40 20 0 80 90 100 110 120 Modulus Length [#points] 40 20 0 -3.5 -3 -2.5 -2 -1.5 -1 H r [nm] 40 20 0 0.02 0.04 0.06 0.08 Fit1 Avg.Abs.Res. 40 20 0 0.05 0.1 0.15 0.2 0.25 Fit1 Max.Abs.Res. 40 20 0 0.2 0.3 0.4 0.5 0.6 0.7 Fit2 Avg.Abs.Res. 1 1.5 2 2.5 3 40 20 0 Fit2 Max.Abs.Res. 0 0.05 0.1 0.15 0.2 0.25 40 20 0 h change [nm/nm] 0 0.05 0.1 0.15 0.2 40 20 0 P change [mN/mN] 4 6 8 10 12 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 40 20 0 0.01 0.015 0.02 0.025 0.03 Fit4 Max.Abs.Res. 40 20 0 0.5 1 1.5 2 2.5 3 P* [mN] 40 20 0 10 15 20 25 30 h* [nm] 0 0.005 0.01 0.015 0.02 40 20 0 dP [mN] 40 20 0 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  26. 26. 400F_ 100micron tip_ test 004 Estat = mean: 72.9889 median: 73.1361 stdev: 1.8000 min: 70.0546 max: 75.9991 Ystat = mean: 0.6103 median: 0.6072 stdev: 0.0260 min: 0.5609 max: 0.6650 Hstat = mean: 26.9273 median: 26.9275 stdev: 0.7568 min: 25.5735 max: 28.3435 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.6 1.4 1.2 1 0.8 0.6 0.4 0.2 0 Ind. Strain Ind. Stress [GPa] Es=69.4253; Bunge=0, 0, 0; Strength=0.6109; Hardening=26.7417 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 2 0 -2 -4 -6 6 -1 0 1 2 3 5 x 10 -8 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 30 25 20 15 10 5 0 P 2/3 h Modulus Fit Data Elastic 0 0.05 0.1 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  27. 27. 400F_ 100micron tip_ test 005 40 20 0 66 68 70 72 74 76 Modulus [GPa] 100 50 0 0.95 0.96 0.97 0.98 0.99 1 R2 40 20 0 60 80 100 120 Modulus Length [#points] 100 50 0 -4 -3 -2 -1 0 H r [nm] 0 0.02 0.04 0.06 0.08 0.1 100 50 0 Fit1 Avg.Abs.Res. 0 0.05 0.1 0.15 0.2 0.25 100 50 0 Fit1 Max.Abs.Res. 0 0.2 0.4 0.6 0.8 100 50 0 Fit2 Avg.Abs.Res. 0 1 2 3 4 40 20 0 Fit2 Max.Abs.Res. 40 20 0 -0.1 0 0.1 0.2 0.3 h change [nm/nm] 0 0.05 0.1 0.15 0.2 40 20 0 P change [mN/mN] 4 6 8 10 12 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 40 20 0 0.01 0.015 0.02 0.025 Fit4 Max.Abs.Res. 0 1 2 3 4 100 50 0 P* [mN] 0 10 20 30 40 100 50 0 h* [nm] 0 0.005 0.01 0.015 0.02 50 0 dP [mN] 40 20 0 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  28. 28. 400F_ 100micron tip_ test 005 Estat = mean: 72.4187 median: 72.3209 stdev: 1.5646 min: 70.0299 max: 75.9694 Ystat = mean: 0.5981 median: 0.5954 stdev: 0.0208 min: 0.5477 max: 0.6574 Hstat = mean: 25.8628 median: 25.7550 stdev: 0.6907 min: 24.7395 max: 27.5316 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=68.8299; Bunge=0, 0, 0; Strength=0.58431; Hardening=25.9528 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 1 2 3 5 x 10 2 0 -2 -4 -6 -8 -10 -12 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 4 40 30 20 10 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  29. 29. 400F_ 100micron tip_ test 006 20 10 0 66 68 70 72 74 76 Modulus [GPa] 200 100 0 0.95 0.96 0.97 0.98 0.99 1 R2 20 10 0 60 70 80 90 100 110 Modulus Length [#points] 40 20 0 -4 -3 -2 -1 0 H r [nm] 0 0.02 0.04 0.06 0.08 40 20 0 Fit1 Avg.Abs.Res. 0 0.05 0.1 0.15 0.2 0.25 40 20 0 Fit1 Max.Abs.Res. 0 0.2 0.4 0.6 0.8 100 50 0 Fit2 Avg.Abs.Res. 0 1 2 3 40 20 0 Fit2 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 0.5 100 50 0 h change [nm/nm] 0 0.1 0.2 0.3 0.4 100 50 0 P change [mN/mN] 5 6 7 8 9 10 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 40 20 0 0.015 0.02 0.025 0.03 Fit4 Max.Abs.Res. 0 1 2 3 4 40 20 0 P* [mN] 0 10 20 30 40 40 20 0 h* [nm] 0 0.005 0.01 0.015 0.02 40 20 0 dP [mN] 40 20 0 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  30. 30. 400F_ 100micron tip_ test 006 Estat = mean: 72.5387 median: 72.3448 stdev: 1.6706 min: 70.0031 max: 75.9708 Ystat = mean: 0.6235 median: 0.6197 stdev: 0.0376 min: 0.5521 max: 0.7019 Hstat = mean: 25.2648 median: 25.1910 stdev: 0.6441 min: 24.1051 max: 26.5741 1.6 1.4 1.2 1 0.8 0.6 0.4 0.2 0 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 Ind. Strain Ind. Stress [GPa] Es=68.9125; Bunge=0, 0, 0; Strength=0.64253; Hardening=25.1394 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 1 2 3 5 x 10 5 0 -5 -10 -15 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 4 40 30 20 10 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  31. 31. 400F_ 100micron tip_ test 007 20 10 0 66 68 70 72 74 76 Modulus [GPa] 40 20 0 0.95 0.96 0.97 0.98 0.99 1 R2 20 10 0 95 100 105 110 115 120 Modulus Length [#points] 20 10 0 -3 -2.5 -2 -1.5 -1 H r [nm] 20 10 0 0.02 0.03 0.04 0.05 0.06 Fit1 Avg.Abs.Res. 20 10 0 0.05 0.1 0.15 0.2 0.25 Fit1 Max.Abs.Res. 0.35 0.4 0.45 0.5 0.55 0.6 20 10 0 Fit2 Avg.Abs.Res. 1 1.5 2 2.5 3 20 10 0 Fit2 Max.Abs.Res. 40 20 0 -0.05 0 0.05 0.1 0.15 h change [nm/nm] 0 0.02 0.04 0.06 0.08 0.1 40 20 0 P change [mN/mN] 5 6 7 8 9 10 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 20 10 0 0.015 0.02 0.025 0.03 Fit4 Max.Abs.Res. 20 10 0 0.5 1 1.5 2 2.5 P* [mN] 20 10 0 10 15 20 25 h* [nm] 0 0.005 0.01 0.015 0.02 20 10 0 dP [mN] 20 10 0 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  32. 32. 400F_ 100micron tip_ test 007 Estat = mean: 72.5940 median: 72.4691 stdev: 1.6808 min: 70.0073 max: 75.9954 Ystat = mean: 0.6301 median: 0.6262 stdev: 0.0239 min: 0.5901 max: 0.6833 Hstat = mean: 24.2083 median: 24.1450 stdev: 0.6232 min: 23.2490 max: 25.4870 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=68.9381; Bunge=0, 0, 0; Strength=0.62268; Hardening=24.145 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 1 2 3 5 x 10 5 0 -5 -10 -15 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 4 50 40 30 20 10 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  33. 33. 400F_ 100micron tip_ test 008 10 5 0 65 70 75 80 Modulus [GPa] 10 5 0 0.94 0.96 0.98 1 R2 10 5 0 70 75 80 85 90 Modulus Length [#points] 20 10 0 -3 -2.5 -2 -1.5 -1 H r [nm] 10 5 0 0.03 0.04 0.05 0.06 Fit1 Avg.Abs.Res. 10 5 0 0.08 0.1 0.12 0.14 0.16 Fit1 Max.Abs.Res. 0.35 0.4 0.45 0.5 10 5 0 Fit2 Avg.Abs.Res. 1 1.5 2 2.5 20 10 0 Fit2 Max.Abs.Res. 0 0.05 0.1 0.15 0.2 20 10 0 h change [nm/nm] 0 0.05 0.1 0.15 0.2 40 20 0 P change [mN/mN] 6 8 10 12 -3 x 10 10 5 0 Fit4 Avg.Abs.Res. 10 5 0 0.018 0.02 0.022 0.024 0.026 Fit4 Max.Abs.Res. 10 5 0 1.4 1.6 1.8 2 2.2 P* [mN] 10 5 0 16 18 20 22 24 h* [nm] 0 0.005 0.01 0.015 0.02 10 5 0 dP [mN] 10 5 0 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  34. 34. 400F_ 100micron tip_ test 008 Estat = mean: 72.8347 median: 72.7764 stdev: 1.7629 min: 70.0515 max: 75.9819 Ystat = mean: 0.6153 median: 0.6150 stdev: 0.0243 min: 0.5745 max: 0.6635 Hstat = mean: 25.5687 median: 25.5641 stdev: 0.6504 min: 24.5436 max: 26.8152 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.6 1.4 1.2 1 0.8 0.6 0.4 0.2 0 Ind. Strain Ind. Stress [GPa] Es=69.3031; Bunge=0, 0, 0; Strength=0.61882; Hardening=25.6051 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 2 0 -2 -4 -6 -8 6 -1 0 1 2 3 5 x 10 -10 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 40 30 20 10 0 -10 P 2/3 h Modulus Fit Data Elastic 0 0.1 0.2 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  35. 35. 400F_ 100micron tip_ test 009 20 10 0 65 70 75 80 Modulus [GPa] 20 10 0 0.94 0.96 0.98 1 R2 40 20 0 90 100 110 120 Modulus Length [#points] 20 10 0 -2 -1.5 -1 -0.5 H r [nm] 40 20 0 0.02 0.03 0.04 0.05 Fit1 Avg.Abs.Res. 20 10 0 0.05 0.1 0.15 Fit1 Max.Abs.Res. 0.35 0.4 0.45 0.5 20 10 0 Fit2 Avg.Abs.Res. 1 1.5 2 2.5 20 10 0 Fit2 Max.Abs.Res. 20 10 0 -0.05 0 0.05 0.1 0.15 h change [nm/nm] 0 0.05 0.1 20 10 0 P change [mN/mN] 4 6 8 10 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 20 10 0 0.015 0.02 0.025 0.03 Fit4 Max.Abs.Res. 20 10 0 0.5 1 1.5 2 P* [mN] 20 10 0 10 15 20 h* [nm] 0 0.005 0.01 0.015 0.02 20 10 0 dP [mN] 40 20 0 0.2 0.4 0.6 0.8 1 dH [nm] effective sample Fit1 Fit2 Fit3
  36. 36. 400F_ 100micron tip_ test 009 Estat = mean: 72.7375 median: 72.5867 stdev: 1.7351 min: 70.0108 max: 75.9380 Ystat = mean: 0.5990 median: 0.5987 stdev: 0.0244 min: 0.5534 max: 0.6502 Hstat = mean: 25.0370 median: 25.0045 stdev: 0.6484 min: 23.9826 max: 26.3593 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=69.186; Bunge=0, 0, 0; Strength=0.60556; Hardening=25.147 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 300 250 200 150 100 50 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 2 0 -2 -4 -6 -8 6 -1 0 1 2 3 5 x 10 -10 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 1 2 3 35 30 25 20 15 10 5 0 P 2/3 h Modulus Fit Data Elastic 0 0.2 0.4 0.6 0.8 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  37. 37. 400F_ 100micron tip_ test 010 20 10 0 65 70 75 80 Modulus [GPa] 20 10 0 0.94 0.96 0.98 1 R2 40 20 0 10 20 30 40 50 Modulus Length [#points] 20 10 0 -2 -1.5 -1 -0.5 H r [nm] 0 0.02 0.04 0.06 40 20 0 Fit1 Avg.Abs.Res. 0 0.05 0.1 0.15 0.2 20 10 0 Fit1 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 20 10 0 Fit2 Avg.Abs.Res. 20 10 0 0.2 0.4 0.6 0.8 1 Fit2 Max.Abs.Res. 20 10 0 0.5 0.6 0.7 0.8 0.9 h change [nm/nm] 40 20 0 0.4 0.6 0.8 1 P change [mN/mN] 20 10 0 0.006 0.008 0.01 0.012 0.014 Fit4 Avg.Abs.Res. 20 10 0 0.015 0.02 0.025 0.03 Fit4 Max.Abs.Res. 0 0.5 1 1.5 20 10 0 P* [mN] 5 10 15 20 25 20 10 0 h* [nm] 0 0.005 0.01 0.015 0.02 20 10 0 dP [mN] 40 20 0 -1 -0.5 0 0.5 dH [nm] effective sample Fit1 Fit2 Fit3
  38. 38. 400F_ 100micron tip_ test 010 Estat = mean: 72.9543 median: 72.9222 stdev: 1.6266 min: 70.0865 max: 75.9163 Ystat = mean: 0.4556 median: 0.4465 stdev: 0.0448 min: 0.3839 max: 0.5389 Hstat = mean: 28.2196 median: 28.1243 stdev: 0.8397 min: 26.5468 max: 29.9858 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1.5 1 0.5 0 Ind. Strain Ind. Stress [GPa] Es=69.3707; Bunge=0, 0, 0; Strength=0.53241; Hardening=27.4405 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 300 250 200 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 0 -2 -4 -6 6 0.5 1 1.5 2 2.5 5 x 10 -8 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 2.5 25 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  39. 39. 525F_ 100micron tip_ test 001 20 10 0 65 70 75 80 Modulus [GPa] 40 20 0 0.94 0.96 0.98 1 R2 40 20 0 80 90 100 110 120 Modulus Length [#points] 20 10 0 -1 -0.8 -0.6 -0.4 -0.2 H r [nm] 20 10 0 0.005 0.01 0.015 0.02 Fit1 Avg.Abs.Res. 20 10 0 0.02 0.03 0.04 0.05 0.06 Fit1 Max.Abs.Res. 40 20 0 0.1 0.15 0.2 0.25 Fit2 Avg.Abs.Res. 0.4 0.5 0.6 0.7 20 10 0 Fit2 Max.Abs.Res. 20 10 0 0.2 0.3 0.4 0.5 h change [nm/nm] 0.2 0.25 0.3 0.35 40 20 0 P change [mN/mN] 7 8 9 10 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 40 20 0 0.02 0.025 0.03 0.035 0.04 Fit4 Max.Abs.Res. 40 20 0 0.05 0.1 0.15 0.2 0.25 P* [mN] 3 4 5 6 7 40 20 0 h* [nm] 0 0.5 1 1.5 2 -3 x 10 20 10 0 dP [mN] 40 20 0 -0.6 -0.4 -0.2 0 0.2 dH [nm] effective sample Fit1 Fit2 Fit3
  40. 40. 525F_ 100micron tip_ test 001 Estat = mean: 72.8279 median: 73.1006 stdev: 1.7629 min: 70.0003 max: 75.9999 Ystat = mean: 0.3439 median: 0.3420 stdev: 0.0158 min: 0.3150 max: 0.3783 Hstat = mean: 17.3318 median: 17.3867 stdev: 0.4754 min: 16.5865 max: 18.4025 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1 0.9 0.8 0.7 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.2875; Bunge=0, 0, 0; Strength=0.34963; Hardening=17.2816 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 200 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 5 x 10 0 -0.5 -1 -1.5 -2 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.2 0.4 0.6 0.8 1 10 8 6 4 2 0 -2 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  41. 41. 525F_ 100micron tip_ test 002 40 20 0 66 68 70 72 74 76 Modulus [GPa] 200 100 0 0.95 0.96 0.97 0.98 0.99 1 R2 100 50 0 50 100 150 Modulus Length [#points] 100 50 0 -1.2 -1 -0.8 -0.6 -0.4 -0.2 H r [nm] 100 50 0 0.005 0.01 0.015 0.02 Fit1 Avg.Abs.Res. 0 0.02 0.04 0.06 0.08 0.1 200 100 0 Fit1 Max.Abs.Res. 100 50 0 0.1 0.15 0.2 0.25 0.3 0.35 Fit2 Avg.Abs.Res. 200 100 0 0.2 0.4 0.6 0.8 1 1.2 Fit2 Max.Abs.Res. 200 100 0 -0.2 0 0.2 0.4 0.6 h change [nm/nm] 0 0.1 0.2 0.3 0.4 200 100 0 P change [mN/mN] 5 6 7 8 9 10 -3 x 10 100 50 0 Fit4 Avg.Abs.Res. 100 50 0 0.01 0.02 0.03 0.04 0.05 0.06 Fit4 Max.Abs.Res. 100 50 0 0.1 0.2 0.3 0.4 0.5 P* [mN] 6 7 8 9 10 11 100 50 0 h* [nm] 0 0.5 1 1.5 2 2.5 -3 x 10 50 0 dP [mN] 100 50 0 -0.4 -0.2 0 0.2 0.4 0.6 dH [nm] effective sample Fit1 Fit2 Fit3
  42. 42. 525F_ 100micron tip_ test 002 Estat = mean: 73.0168 median: 72.9951 stdev: 1.7580 min: 70.0013 max: 75.9956 Ystat = mean: 0.3923 median: 0.3923 stdev: 0.0185 min: 0.3468 max: 0.4306 Hstat = mean: 18.0153 median: 17.8977 stdev: 0.6708 min: 17.0777 max: 19.5268 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1 0.8 0.6 0.4 0.2 0 Ind. Strain Ind. Stress [GPa] Es=69.4679; Bunge=0, 0, 0; Strength=0.36933; Hardening=18.023 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 500 1000 250 200 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 5 x 10 0 -0.5 -1 -1.5 -2 -2.5 -3 -3.5 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 20 15 10 5 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  43. 43. 525F_ 100micron tip_ test 003 20 10 0 65 70 75 80 Modulus [GPa] 50 0 0.94 0.96 0.98 1 R2 20 10 0 50 100 150 Modulus Length [#points] 20 10 0 -0.9 -0.8 -0.7 -0.6 -0.5 H r [nm] 40 20 0 0.005 0.01 0.015 Fit1 Avg.Abs.Res. 40 20 0 0.025 0.03 0.035 0.04 0.045 Fit1 Max.Abs.Res. 40 20 0 0.1 0.11 0.12 0.13 Fit2 Avg.Abs.Res. 0.4 0.5 0.6 0.7 40 20 0 Fit2 Max.Abs.Res. 40 20 0 0.1 0.2 0.3 0.4 0.5 h change [nm/nm] 20 10 0 0.1 0.2 0.3 0.4 0.5 P change [mN/mN] 6 7 8 9 10 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 100 50 0 0.025 0.03 0.035 0.04 Fit4 Max.Abs.Res. 20 10 0 0.12 0.14 0.16 0.18 P* [mN] 20 10 0 4.5 5 5.5 6 h* [nm] 0 0.5 1 1.5 2 -3 x 10 20 10 0 dP [mN] 40 20 0 -1 -0.5 0 0.5 dH [nm] effective sample Fit1 Fit2 Fit3
  44. 44. 525F_ 100micron tip_ test 003 Estat = mean: 72.8329 median: 72.6625 stdev: 1.6899 min: 70.0091 max: 75.9662 Ystat = mean: 0.4241 median: 0.4226 stdev: 0.0182 min: 0.3933 max: 0.4577 Hstat = mean: 17.1184 median: 17.0781 stdev: 0.4141 min: 16.4184 max: 17.9105 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1 0.8 0.6 0.4 0.2 0 Ind. Strain Ind. Stress [GPa] Es=69.3119; Bunge=0, 0, 0; Strength=0.42218; Hardening=17.1288 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 250 200 150 100 50 0 -500 0 500 1000 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 5 0 5 10 15 4 x 10 2 0 -2 -4 -6 -8 -10 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.2 0.4 0.6 0.8 5 4 3 2 1 0 -1 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  45. 45. 525F_ 100micron tip_ test 004 30 20 10 65 70 75 80 Modulus [GPa] 200 100 0 0.94 0.96 0.98 1 R2 0 50 100 150 50 0 Modulus Length [#points] 100 50 0 -1.5 -1 -0.5 0 H r [nm] 0 0.01 0.02 0.03 100 50 0 Fit1 Avg.Abs.Res. 0 0.02 0.04 0.06 0.08 100 50 0 Fit1 Max.Abs.Res. 100 50 0 0.05 0.1 0.15 0.2 0.25 Fit2 Avg.Abs.Res. 50 0 0.2 0.4 0.6 0.8 1 Fit2 Max.Abs.Res. 50 0 0.2 0.4 0.6 0.8 h change [nm/nm] 50 0 0.1 0.2 0.3 0.4 0.5 P change [mN/mN] 4 6 8 10 -3 x 10 100 50 0 Fit4 Avg.Abs.Res. 100 50 0 0.01 0.02 0.03 0.04 Fit4 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 100 50 0 P* [mN] 6 8 10 12 100 50 0 h* [nm] 0 1 2 3 4 -3 x 10 40 20 0 dP [mN] 100 50 0 -1 -0.5 0 0.5 dH [nm] effective sample Fit1 Fit2 Fit3
  46. 46. 525F_ 100micron tip_ test 004 Estat = mean: 72.9655 median: 72.8722 stdev: 1.7495 min: 70.0414 max: 75.9761 Ystat = mean: 0.3900 median: 0.3888 stdev: 0.0169 min: 0.3590 max: 0.4202 Hstat = mean: 17.9959 median: 17.9677 stdev: 0.4532 min: 17.2153 max: 18.7965 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1 0.8 0.6 0.4 0.2 0 Ind. Strain Ind. Stress [GPa] Es=69.4561; Bunge=0, 0, 0; Strength=0.38674; Hardening=18.0079 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 200 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 5 x 10 0 -1 -2 -3 -4 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  47. 47. 525F_ 100micron tip_ test 005 20 10 0 66 68 70 72 74 76 Modulus [GPa] 40 20 0 0.95 0.96 0.97 0.98 0.99 1 R2 40 20 0 70 80 90 100 110 120 Modulus Length [#points] 40 20 0 -1.5 -1 -0.5 0 H r [nm] 40 20 0 0.005 0.01 0.015 0.02 Fit1 Avg.Abs.Res. 40 20 0 0.02 0.04 0.06 0.08 0.1 Fit1 Max.Abs.Res. 50 0 0.1 0.15 0.2 0.25 0.3 0.35 Fit2 Avg.Abs.Res. 40 20 0 0.2 0.4 0.6 0.8 1 1.2 Fit2 Max.Abs.Res. 20 10 0 0.2 0.3 0.4 0.5 h change [nm/nm] 0.2 0.25 0.3 0.35 40 20 0 P change [mN/mN] 7 8 9 10 -3 x 10 40 20 0 Fit4 Avg.Abs.Res. 50 0 0.02 0.025 0.03 0.035 0.04 Fit4 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 0.5 50 0 P* [mN] 2 4 6 8 10 40 20 0 h* [nm] 0 1 2 3 4 5 -3 x 10 40 20 0 dP [mN] 40 20 0 -0.6 -0.4 -0.2 0 0.2 0.4 dH [nm] effective sample Fit1 Fit2 Fit3
  48. 48. 525F_ 100micron tip_ test 005 Estat = mean: 72.9610 median: 73.1697 stdev: 1.8039 min: 70.0003 max: 75.9999 Ystat = mean: 0.3449 median: 0.3440 stdev: 0.0155 min: 0.3150 max: 0.3783 Hstat = mean: 17.3682 median: 17.4043 stdev: 0.4815 min: 16.5865 max: 18.4025 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 1 0.9 0.8 0.7 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.4314; Bunge=0, 0, 0; Strength=0.3375; Hardening=17.4237 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 200 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 5 x 10 0 -0.5 -1 -1.5 -2 -2.5 -3 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  49. 49. 650F_ 100micron tip_ test 002 20 10 0 65 70 75 80 Modulus [GPa] 50 0 0.98 0.99 1 1.01 R2 20 10 0 20 40 60 80 Modulus Length [#points] 20 10 0 -2 -1 0 1 H r [nm] 40 20 0 0.08 0.1 0.12 0.14 0.16 Fit1 Avg.Abs.Res. 40 20 0 0.2 0.3 0.4 0.5 Fit1 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 20 10 0 Fit2 Avg.Abs.Res. 0 0.5 1 1.5 20 10 0 Fit2 Max.Abs.Res. 20 10 0 0.7 0.8 0.9 1 h change [nm/nm] 40 20 0 0.4 0.5 0.6 0.7 0.8 P change [mN/mN] 20 10 0 0.02 0.03 0.04 0.05 Fit4 Avg.Abs.Res. 20 10 0 0.04 0.05 0.06 0.07 0.08 Fit4 Max.Abs.Res. 0.8 1 1.2 1.4 20 10 0 P* [mN] 20 10 0 30 35 40 45 h* [nm] 0 0.005 0.01 0.015 20 10 0 dP [mN] 20 10 0 -0.5 0 0.5 1 1.5 dH [nm] effective sample Fit1 Fit2 Fit3
  50. 50. 650F_ 100micron tip_ test 002 Estat = mean: 73.0756 median: 72.9917 stdev: 1.6628 min: 70.1255 max: 75.9698 Ystat = mean: 0.2518 median: 0.2515 stdev: 0.0119 min: 0.2208 max: 0.2790 Hstat = mean: 12.9052 median: 12.8873 stdev: 0.7722 min: 11.7981 max: 14.2977 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.7 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.4988; Bunge=0, 0, 0; Strength=0.25718; Hardening=12.4377 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 140 120 100 80 60 40 20 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 1 2 3 5 x 10 0 -2 -4 -6 -8 -10 -12 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 25 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  51. 51. 650F_ 100micron tip_ test 003
  52. 52. 650F_ 100micron tip_ test 003 Estat = mean: 72.8141 median: 72.5877 stdev: 1.7410 min: 70.0232 max: 75.9629 Ystat = mean: 0.2503 median: 0.2504 stdev: 0.0100 min: 0.2326 max: 0.2741 Hstat = mean: 13.3240 median: 13.2591 stdev: 0.4620 min: 12.0619 max: 14.2475 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.8 0.7 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.2711; Bunge=0, 0, 0; Strength=0.25215; Hardening=13.2591 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 500 1000 150 100 50 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 1 2 3 5 x 10 0 -2 -4 -6 -8 -10 -12 -14 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 25 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 0.04 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  53. 53. 650F_ 100micron tip_ test 004 10 5 0 65 70 75 80 Modulus [GPa] 40 20 0 0.98 0.99 1 1.01 R2 20 10 0 20 40 60 80 Modulus Length [#points] 20 10 0 -2 -1 0 1 H r [nm] 40 20 0 0.1 0.12 0.14 0.16 Fit1 Avg.Abs.Res. 20 10 0 0.25 0.3 0.35 0.4 0.45 Fit1 Max.Abs.Res. 0 0.1 0.2 0.3 0.4 20 10 0 Fit2 Avg.Abs.Res. 0 0.5 1 1.5 20 10 0 Fit2 Max.Abs.Res. 10 5 0 0.75 0.8 0.85 0.9 0.95 h change [nm/nm] 20 10 0 0.4 0.5 0.6 0.7 0.8 P change [mN/mN] 10 5 0 0.02 0.03 0.04 0.05 Fit4 Avg.Abs.Res. 10 5 0 0.045 0.05 0.055 0.06 Fit4 Max.Abs.Res. 10 5 0 0.7 0.8 0.9 1 P* [mN] 10 5 0 54 56 58 60 h* [nm] 0 0.005 0.01 20 10 0 dP [mN] 20 10 0 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  54. 54. 650F_ 100micron tip_ test 004 Estat = mean: 72.7263 median: 72.4234 stdev: 1.7910 min: 70.0506 max: 75.9400 Ystat = mean: 0.2271 median: 0.2261 stdev: 0.0108 min: 0.1959 max: 0.2459 Hstat = mean: 12.3714 median: 12.0507 stdev: 0.6598 min: 11.5263 max: 13.4687 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.7 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.1896; Bunge=0, 0, 0; Strength=0.23049; Hardening=12.0506 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 140 120 100 80 60 40 20 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 1 2 3 5 x 10 0 -2 -4 -6 -8 -10 -12 -14 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 25 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  55. 55. 650F_ 100micron tip_ test 005 10 5 0 65 70 75 80 Modulus [GPa] 40 20 0 0.96 0.98 1 1.02 R2 10 5 0 20 40 60 80 Modulus Length [#points] 10 5 0 -1 -0.5 0 0.5 H r [nm] 20 10 0 0.08 0.1 0.12 0.14 0.16 Fit1 Avg.Abs.Res. 20 10 0 0.2 0.25 0.3 0.35 0.4 Fit1 Max.Abs.Res. 10 5 0 0.05 0.1 0.15 0.2 0.25 Fit2 Avg.Abs.Res. 0 0.5 1 20 10 0 Fit2 Max.Abs.Res. 10 5 0 0.75 0.8 0.85 0.9 0.95 h change [nm/nm] 10 5 0 0.4 0.5 0.6 0.7 0.8 P change [mN/mN] 10 5 0 0.025 0.03 0.035 0.04 0.045 Fit4 Avg.Abs.Res. 10 5 0 0.05 0.055 0.06 0.065 Fit4 Max.Abs.Res. 10 5 0 0.55 0.6 0.65 0.7 0.75 P* [mN] 10 5 0 31 32 33 34 35 h* [nm] 0 2 4 6 8 -3 x 10 10 5 0 dP [mN] 10 5 0 -0.5 0 0.5 1 dH [nm] effective sample Fit1 Fit2 Fit3
  56. 56. 650F_ 100micron tip_ test 005 Estat = mean: 73.0497 median: 72.7548 stdev: 1.8111 min: 70.0597 max: 75.9970 Ystat = mean: 0.2244 median: 0.2263 stdev: 0.0123 min: 0.1897 max: 0.2476 Hstat = mean: 13.1493 median: 13.0770 stdev: 0.4404 min: 12.2847 max: 13.9221 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.467; Bunge=0, 0, 0; Strength=0.23406; Hardening=12.931 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 100 80 60 40 20 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 2.5 5 x 10 0 -2 -4 -6 -8 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  57. 57. 650F_ 100micron tip_ test 006 20 10 0 66 68 70 72 74 76 Modulus [GPa] 40 20 0 0.95 0.96 0.97 0.98 0.99 1 R2 20 10 0 20 25 30 35 40 45 Modulus Length [#points] 20 10 0 -1 -0.5 0 0.5 1 H r [nm] 20 10 0 0.1 0.2 0.3 0.4 0.5 Fit1 Avg.Abs.Res. 0 0.5 1 1.5 2 20 10 0 Fit1 Max.Abs.Res. 20 10 0 0.1 0.2 0.3 0.4 0.5 0.6 Fit2 Avg.Abs.Res. 0 0.5 1 1.5 2 20 10 0 Fit2 Max.Abs.Res. 40 20 0 0.75 0.8 0.85 0.9 0.95 h change [nm/nm] 0.65 0.7 0.75 0.8 20 10 0 P change [mN/mN] 20 10 0 0.045 0.05 0.055 0.06 0.065 0.07 Fit4 Avg.Abs.Res. 20 10 0 0.06 0.07 0.08 0.09 0.1 0.11 Fit4 Max.Abs.Res. 0 1 2 3 4 5 20 10 0 P* [mN] 20 10 0 60 70 80 90 100 110 h* [nm] 0 0.01 0.02 0.03 20 10 0 dP [mN] 0 0.5 1 1.5 2 2.5 20 10 0 dH [nm] effective sample Fit1 Fit2 Fit3
  58. 58. 650F_ 100micron tip_ test 006 Estat = mean: 72.5025 median: 72.0208 stdev: 1.7646 min: 70.0303 max: 75.9951 Ystat = mean: 0.1528 median: 0.1565 stdev: 0.0120 min: 0.1219 max: 0.1704 Hstat = mean: 14.1212 median: 13.9646 stdev: 0.8057 min: 12.9491 max: 15.8711 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.7 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=68.9422; Bunge=0, 0, 0; Strength=0.16582; Hardening=13.5432 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 140 120 100 80 60 40 20 0 -200 0 200 400 600 800 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 7 0 1 2 3 4 5 x 10 0.5 0 -0.5 -1 -1.5 -2 -2.5 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 2 25 20 15 10 5 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  59. 59. 775F_ 100micron tip_ test 002 10 5 0 66 68 70 72 74 76 Modulus [GPa] 20 10 0 0.95 0.96 0.97 0.98 0.99 1 R2 10 5 0 30 35 40 45 50 55 Modulus Length [#points] 10 5 0 -1 -0.5 0 0.5 1 H r [nm] 20 10 0 0.08 0.1 0.12 0.14 0.16 Fit1 Avg.Abs.Res. 0.3 0.32 0.34 0.36 0.38 20 10 0 Fit1 Max.Abs.Res. 10 5 0 0.1 0.15 0.2 0.25 Fit2 Avg.Abs.Res. 20 10 0 0.2 0.4 0.6 0.8 1 Fit2 Max.Abs.Res. 10 5 0 0.86 0.88 0.9 0.92 0.94 h change [nm/nm] 10 5 0 0.55 0.6 0.65 0.7 0.75 P change [mN/mN] 10 5 0 0.02 0.03 0.04 0.05 0.06 0.07 Fit4 Avg.Abs.Res. 20 10 0 0.04 0.06 0.08 0.1 Fit4 Max.Abs.Res. 10 5 0 0.5 0.6 0.7 0.8 0.9 1 P* [mN] 10 5 0 56 58 60 62 64 66 h* [nm] 0 0.002 0.004 0.006 0.008 0.01 10 5 0 dP [mN] 10 5 0 -0.5 0 0.5 1 1.5 2 dH [nm] effective sample Fit1 Fit2 Fit3
  60. 60. 775F_ 100micron tip_ test 002 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.0392; Bunge=0, 0, 0; Strength=0.15987; Hardening=11.39 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 120 100 80 60 40 20 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 2.5 5 x 10 0 -2 -4 -6 -8 -10 -12 -14 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 20 15 10 5 0 -5 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 8000 6000 4000 2000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic Estat = mean: 72.6774 median: 72.4660 stdev: 1.5328 min: 70.1452 max: 75.7897 Ystat = mean: 0.1801 median: 0.1808 stdev: 0.0080 min: 0.1588 max: 0.2022 Hstat = mean: 10.8999 median: 10.8444 stdev: 0.3716 min: 10.1605 max: 11.7637
  61. 61. 775F_ 100micron tip_ test 004 10 5 0 66 68 70 72 74 76 Modulus [GPa] 20 10 0 0.96 0.97 0.98 0.99 1 1.01 R2 10 5 0 20 30 40 50 60 70 Modulus Length [#points] 10 5 0 -1.5 -1 -0.5 0 0.5 1 H r [nm] 10 5 0 0.1 0.12 0.14 0.16 Fit1 Avg.Abs.Res. 10 5 0 0.25 0.3 0.35 0.4 0.45 Fit1 Max.Abs.Res. 10 5 0 0.1 0.15 0.2 0.25 Fit2 Avg.Abs.Res. 0.4 0.5 0.6 0.7 10 5 0 Fit2 Max.Abs.Res. 4 2 0 0.8 0.85 0.9 0.95 1 h change [nm/nm] 10 5 0 0.5 0.6 0.7 0.8 0.9 P change [mN/mN] 20 10 0 0.02 0.03 0.04 0.05 0.06 0.07 Fit4 Avg.Abs.Res. 20 10 0 0.04 0.05 0.06 0.07 0.08 0.09 Fit4 Max.Abs.Res. 0.7 0.8 0.9 1 1.1 20 10 0 P* [mN] 10 5 0 44 46 48 50 52 54 h* [nm] 0 0.002 0.004 0.006 0.008 0.01 10 5 0 dP [mN] 10 5 0 -1 -0.5 0 0.5 1 1.5 dH [nm] effective sample Fit1 Fit2 Fit3
  62. 62. 775F_ 100micron tip_ test 004 Estat = mean: 72.9440 median: 72.5348 stdev: 1.7310 min: 70.2726 max: 75.8985 Ystat = mean: 0.1815 median: 0.1793 stdev: 0.0162 min: 0.1483 max: 0.2122 Hstat = mean: 11.4562 median: 11.0910 stdev: 0.7168 min: 10.4900 max: 12.6142 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.6 0.5 0.4 0.3 0.2 0.1 0 Ind. Strain Ind. Stress [GPa] Es=69.1715; Bunge=0, 0, 0; Strength=0.18232; Hardening=10.8001 Stress-Strain Modulus Line Hardening Fit Strain Offset Modulus Fit Data Hardening Fit Data Yield Point 0 200 400 600 800 120 100 80 60 40 20 0 displacement / nm load / mN Load Vs. Displacement Raw Data 0 Pt. Data 6 0 0.5 1 1.5 2 2.5 5 x 10 0 -2 -4 -6 -8 -10 -12 x 10 S P2/3-Sh Zero Point Fit Raw Data 0 Pt. Data 0 0.5 1 1.5 20 15 10 5 0 P 2/3 h Modulus Fit Data Elastic 0 0.01 0.02 0.03 7000 6000 5000 4000 3000 2000 1000 0 Strain Contact Radius / nm Strain Vs. Contact Radius Data Elastic
  63. 63. 775F_ 100micron tip_ test 005
  64. 64. 775F_ 100micron tip_ test 005 Estat = mean: 73.0240 median: 73.0903 stdev: 1.7293 min: 70.0061 max: 75.9250 Ystat = mean: 0.2102 median: 0.2100 stdev: 0.0102 min: 0.1834 max: 0.2314 Hstat = mean: 9.9928 median: 9.9663 stdev: 0.2857 min: 9.4651 max: 10.6556
  65. 65. 775F_ 100micron tip_ test 007
  66. 66. 775F_ 100micron tip_ test 007
  67. 67. 775F_ 100micron tip_ test 010
  68. 68. 775F_ 100micron tip_ test 010
  69. 69. Elastic module Yield strength (GPa) Hardening As received 400 F 55.73153 0.422567 20.59428 525 F 56.33968 0.2724 14.30632 650 F 775 F

×